A high-strength aging-resistant porcelain insulator

By using the technology of modified nano-silica and magnesium element layers in ceramic insulators, a loose porous structure and mullite crystals are formed, which solves the problems of brittleness and low reliability of ceramic insulators, and improves the mechanical strength and resistance of porcelain insulators. Aging performance, suitable for UHV transmission systems.

CN116978643BActive Publication Date: 2024-10-22JIANGXI LIHUA ELECTRIC PORCELAIN MFG CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310900727.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-21
Publication Date
2024-10-22
Estimated Expiration
2043-07-21

AI Technical Summary

Technical Problem

Ceramic insulators are highly brittle and have low reliability in UHV transmission systems, resulting in reduced strength, interface breakdown and other problems, shortening service life and increasing maintenance costs, affecting the normal operation of the transmission network.

Method used

Using a porcelain core including alumina, clay, potassium feldspar, zirconia, modified nano-silica, titanium dioxide, bentonite and dolomite powder, and using a calcium-doped silica powder preparation method to form a loose porous structure to inhibit oxidation Aluminum phase transformation increases the movement potential energy of aluminum atoms during the sintering process, enhances the thermal stability and mechanical strength of the material, and promotes the combination of alumina and silicon dioxide through the magnesium element layer to form a mullite crystal structure, improving the strength of the porcelain body. Aging resistance.

Benefits of technology

It improves the flexural strength and breakdown voltage of porcelain insulators, enhances the safety and durability of the insulators, reduces the failure rate, and shows good aging resistance in areas with large temperature changes.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a high-strength aging-resistant porcelain insulator, comprising a porcelain core and an umbrella skirt, wherein the umbrella skirt is mounted on the outside of the porcelain core, and steel caps are bonded on both sides of the porcelain core. The raw materials of the porcelain core include: alumina, clay, potassium feldspar, zirconium oxide, modified nano-silicon dioxide, titanium dioxide, bentonite and dolomite powder. The porcelain core for porcelain insulators prepared by the method of the invention has a high flexural strength breakdown voltage, improves the safety and durability of the insulator, and reduces the failure rate of the porcelain insulator. At the same time, it will not crack after repeated freezing and thawing, has good aging resistance, and is suitable for use in areas with large temperature changes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of insulator materials, and in particular to a high-strength aging-resistant porcelain insulator. Background Art

[0002] In recent years, with the rapid advancement of national urban construction, the UHV transmission industry and technology have also developed rapidly. Since the first ±800kV transmission project in China was put into operation in 2010, after more than ten years of continuous efforts, my country has built the world's largest UHV transmission network. Insulators play an insulating and connecting supporting role in the entire UHV DC transmission system. As an important part of DC transmission, the higher the insulator strength level, the more conducive it is to ultra-long-distance transmission of electricity. Insulators with high strength levels can withstand the weight of longer conductors, thereby reducing the number of elevated towers along the entire transmission line and improving economic benefits. At present, the insulators used in transmission lines are made of three materials: ceramic, glass and composite. Ceramic insulators have the advantages of high mechanical strength, stable chemical properties, good insulation performance and good corrosion resistance, making them the most widely used in the insulator industry. However, ceramic insulators are brittle and have low reliability. During operation, problems such as reduced strength and interface breakdown may occur, which greatly shortens the service life of ceramic insulators. At the same time, it will increase the maintenance cost of insulators and affect the normal operation of the railway power grid. Summary of the invention

[0003] To this end, the present invention provides a high-strength aging-resistant porcelain insulator, comprising a porcelain core and an shed, wherein the shed is mounted on the outside of the porcelain core, and steel caps are bonded on both sides of the porcelain core. The raw materials of the porcelain core include: alumina, clay, potassium feldspar, zirconium oxide, modified nano-silicon dioxide, titanium dioxide, bentonite and dolomite powder; the preparation method of the modified nano-silicon dioxide is:

[0004] (1) in a reaction kettle, a mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol, a mixed aqueous solution of calcium nitrate and urea, and a composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol are prepared; the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol is stirred, and the mixed aqueous solution of calcium nitrate and urea is first added to the solution during the stirring process, and the solution is stirred for more than 30 minutes after the addition is completed, and then the composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol is added dropwise to the solution under stirring to obtain a mixed solution, and the mixed solution is stirred for more than 30 minutes, and then the reaction kettle is closed, heated to 120±5° C. and kept warm for more than 8 hours, and then air-cooled to room temperature after the insulation is completed, and the reaction kettle is opened for solid-liquid separation, and the solid phase is washed twice with ethanol and deionized water, respectively, and dried at 80° C. for more than 20 minutes, and then calcined at 550° C. for 5-6 hours, and air-cooled to room temperature to obtain a doped solid phase;

[0005] (2) preparing a mixed aqueous solution of magnesium chloride and ethanol, keeping the solution constant temperature at 60±3° C. in a water bath, stirring the solution at the constant temperature, adding oleic acid to the solution under stirring, and continuing to stir the solution at a constant temperature of 60±3° C. for more than 30 minutes after the addition is completed, and then adding the doped solid phase to the solution under stirring to form a suspension, and continuing to stir the suspension at a constant temperature of 60±3° C. for more than 10 minutes after the addition is completed, and then dropping sodium hydroxide solution into the suspension under stirring, and continuing to stir the suspension at a constant temperature for more than 40 minutes after the addition is completed, air cooling to room temperature, solid-liquid separation, washing the solid phase with ethanol and deionized water twice each, and drying to obtain a primary modified powder;

[0006] (3) preparing a methanol solution of 3,4-dihydroxybenzaldehyde, stirring the methanol solution of 3,4-dihydroxybenzaldehyde, adding p-phenylenediamine to the solution under stirring, and continuing to stir the solution for more than 10 hours after the addition is completed, adding the primary modified powder to the solution after the addition is completed, and continuing to stir the solution for more than 30 minutes after the addition is completed, then separating the solid and the liquid, and drying the solid phase to obtain the modified nano-silica.

[0007] Furthermore, the raw materials of the porcelain core are calculated by weight as follows: 50 parts of alumina, 16-20 parts of clay, 12-15 parts of potassium feldspar, 8-10 parts of zirconium oxide, 20-26 parts of modified nano-silicon dioxide, 3-8 parts of titanium dioxide, 6-10 parts of bentonite, and 2-5 parts of dolomite powder; each raw material is a powder that passes through a 400-mesh sieve.

[0008] Furthermore, in the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol, the concentration of hexadecyltrimethylammonium bromide is 3-4 g / 100 mL, the concentration of urea is 1.6-2.6 g / 100 mL, the concentration of ethylene glycol is 10-20 mL / 100 mL, and the solvent is water; in the mixed aqueous solution of calcium nitrate and urea, the concentration of calcium nitrate is 2.0-2.5 g / 100 mL, the concentration of urea is 0.8-1 g / 100 mL, and the solvent is water; in the composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol, the mixing ratio of tetraethyl orthosilicate, cyclohexane and n-pentanol is tetraethyl orthosilicate: cyclohexane: n-pentanol = 6-7 g: 100 mL: 4-5 mL.

[0009] Furthermore, the volume ratio of the mixed aqueous solution of calcium nitrate and urea and the composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol to the mixed aqueous solution of cetyltrimethylammonium bromide, urea and ethylene glycol is: the mixed aqueous solution of calcium nitrate and urea: the composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol: the mixed aqueous solution of cetyltrimethylammonium bromide, urea and ethylene glycol = 3:1:10.

[0010] Furthermore, in the step (2), in the mixed aqueous solution of magnesium chloride and ethanol, the concentration of magnesium chloride is 5-7 g / 100 mL, and the volume percentage of ethanol is 60%-70%; the mass ratio of the added mass of oleic acid to the mixed aqueous solution of magnesium chloride and ethanol is oleic acid: mixed aqueous solution of magnesium chloride and ethanol = 2-3:100; the solid-liquid mass ratio of adding the doped solid phase to the solution to form a suspension is solid / liquid = 1:20; the concentration of sodium hydroxide in the sodium hydroxide solution is 1 mol / L, and the volume ratio of the added volume of the sodium hydroxide solution to the suspension is sodium hydroxide solution: suspension = 1:5.

[0011] Furthermore, in the step (3), in the methanol solution of 3,4-dihydroxybenzaldehyde, the concentration of 3,4-dihydroxybenzaldehyde is 10-12 g / 100 mL, and the solvent is methanol; the amount ratio of the added mass of p-phenylenediamine to the methanol solution of 3,4-dihydroxybenzaldehyde is p-phenylenediamine / methanol solution of 3,4-dihydroxybenzaldehyde=3-5 g / 100 mL, and the solid-liquid mass ratio of the primary modified powder added to the solution is solid / liquid=1:20.

[0012] The present invention also discloses a method for preparing the above-mentioned porcelain insulator, comprising the following steps:

[0013] Step 1, weighing the raw materials according to the weight proportions, mixing the raw materials to form a mixed powder, and adding water to the mixed powder in a ball mill to obtain a slurry;

[0014] Step 2, dewatering the slurry by filter pressing, adjusting the water content of the slurry to 25wt%, and then pressing it into an insulator blank, drying the blank at 100°C for 20h, then heating it to 400°C at a heating rate of 10°C / min and calcining it for 1h, then heating it to 1200°C at a heating rate of 5°C / min and sintering it for 1h, then heating it to 1280°C at a heating rate of 2°C / min and sintering it for 2h, then cooling it to 1000°C at a cooling rate of 2°C / min and keeping it for 30min, then cooling it to 600°C at a cooling rate of 5°C / min and keeping it for 30min, then cooling it to 200°C at a cooling rate of 10°C / min, taking it out and air cooling it to room temperature to obtain the porcelain insulator.

[0015] Furthermore, the ball milling process is as follows: the weight ratio of balls to water and materials is balls: water: materials = 1:1.2:1, the ball milling speed is 100 r / min, the planetary ball mill is used, and the ball milling time is 10 h.

[0016] The mechanism of the technical solution of the present invention is: the present invention obtains a loose and porous microparticle structure containing calcium elements by calcium doping silica powder, and the doping element changes the silica crystal structure, so that calcium, silicon and other elements are more easily diffused during the sintering process, and the loose and porous structure is easy to adsorb with alumina. On the one hand, silica is used to inhibit the phase transformation of alumina during the sintering process. At the same time, due to the accelerated diffusion of calcium and silicon elements, the ion hole density on the surface of alumina is reduced, forming a steric hindrance, increasing the mobile potential energy of aluminum atoms during the sintering process, inhibiting its phase transformation process, thereby better improving the thermal stability of alumina, avoiding the lattice distortion and microcracks caused by the phase transformation of alumina, and improving the overall strength and aging resistance of the material. A magnesium-containing layer is formed on the surface of silica, and the dissolution of alumina by the magnesium-containing layer during the calcination process promotes alumina and silica to form a mullite crystal structure, improves the bonding strength and density of alumina and silica particles, and further improves the mechanical strength and aging resistance of the porcelain body. Subsequently, boron-containing macromolecular structures are adsorbed on the surface of silica particles, which reduces the agglomeration of silica particles during the preparation of ceramic green sheets. At the same time, the boron-containing macromolecules are calcined to generate boron oxide during the sintering process. Boron oxide is easily fused with silicon oxide and aluminum oxide to form a melt with a lower melting temperature. Due to the high fluidity of the melt, the holes and microcracks generated by phase change can be filled during the sintering process. At the same time, boron oxide is a glass network former, which is beneficial to improve the thermal and chemical stability of the material after sintering.

[0017] The beneficial effects of the present invention are as follows: the porcelain core for porcelain insulators prepared by the method of the present invention has a high flexural strength breakdown voltage, improves the safety and durability of the insulator, and reduces the failure rate of the porcelain insulator. At the same time, it will not crack after repeated freezing and thawing, has good aging resistance, and is suitable for use in areas with large temperature changes. DETAILED DESCRIPTION

[0018] The present invention will be further described below in conjunction with the embodiments.

[0019] Example 1

[0020] A high-strength aging-resistant porcelain insulator comprises a porcelain core and an shed, wherein the shed is mounted on the outside of the porcelain core, and steel caps are bonded to both sides of the porcelain core. The raw materials of the porcelain core comprise: alumina, clay, potassium feldspar, zirconium oxide, modified nano silicon dioxide, titanium dioxide, bentonite and dolomite powder; the raw materials of the porcelain core are as follows by weight: 50 parts of alumina, 16 parts of clay, 12 parts of potassium feldspar, 8 parts of zirconium oxide, 20 parts of modified nano silicon dioxide, 3 parts of titanium dioxide, 6 parts of bentonite and 2 parts of dolomite powder; all raw materials are powders that pass through a 400-mesh sieve; the preparation method of the modified nano silicon dioxide is as follows:

[0021] (1) In a reaction kettle, a mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol, a mixed aqueous solution of calcium nitrate and urea, and a composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol are prepared; in the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol, the concentration of hexadecyltrimethylammonium bromide is 3 g / 100 mL, the concentration of urea is 1.6 g / 100 mL, the concentration of ethylene glycol is 10 mL / 100 mL, and the solvent is water. ; In the mixed aqueous solution of calcium nitrate and urea, the concentration of calcium nitrate is 2.0 g / 100 mL, the concentration of urea is 0.8 g / 100 mL, and the solvent is water; in the composite solution of tetraethyl orthosilicate, cyclohexane, and n-pentanol, the mixing ratio of tetraethyl orthosilicate, cyclohexane, and n-pentanol is tetraethyl orthosilicate: cyclohexane: n-pentanol = 6 g: 100 mL: 4 mL; the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea, and ethylene glycol is stirred at 50 r / min, and during the stirring process The mixed aqueous solution of calcium nitrate and urea is first added to the solution, and the solution is stirred for 30 minutes after the addition is completed. Then, the composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol is added dropwise to the solution under stirring to obtain a mixed solution, and the mixed solution is stirred for 30 minutes. The volume ratio of the mixed aqueous solution of calcium nitrate and urea and the composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol to the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol is 1:1. A mixed aqueous solution of calcium and urea: a composite solution of tetraethyl orthosilicate, cyclohexane, and n-pentanol: a mixed aqueous solution of hexadecyltrimethylammonium bromide, urea, and ethylene glycol = 3:1:10; then the reactor is closed, heated to 120±5°C and kept warm for 8 hours, air-cooled to room temperature after the insulation is completed, the reactor is opened, the solid-liquid separation is performed, the solid phase is washed twice with ethanol and deionized water, dried at 80°C for 20 minutes, and then calcined at 550°C for 5 hours, and air-cooled to room temperature to obtain a doped solid phase;

[0022] (2) preparing a mixed aqueous solution of magnesium chloride and ethanol, wherein the concentration of magnesium chloride is 5 g / 100 mL and the volume percentage of ethanol is 60%; placing the solution in a water bath at a constant temperature of 60±3° C., stirring the solution at a constant temperature of 50 r / min, adding oleic acid to the solution under stirring, wherein the mass ratio of the added oleic acid to the mixed aqueous solution of magnesium chloride and ethanol is oleic acid: mixed aqueous solution of magnesium chloride and ethanol = 2:100; after the addition is completed, the solution is stirred at a constant temperature of 60±3° C. for 30 min, and then the doped solid phase is added to the solution under stirring to form a suspension, and The doped solid phase is added to the solution to form a suspension with a solid-liquid mass ratio of solid / liquid = 1:20; after the addition is completed, the suspension is stirred at a constant temperature of 60±3°C and 50r / min for 10min, and then a sodium hydroxide solution is added dropwise to the suspension under stirring, wherein the concentration of sodium hydroxide in the sodium hydroxide solution is 1mol / L, and the volume ratio of the added volume of the sodium hydroxide solution to the suspension is sodium hydroxide solution: suspension = 1:5; after the addition is completed, the suspension is stirred at a constant temperature for 40min, air-cooled to room temperature, solid-liquid separated, the solid phase is washed twice with ethanol and deionized water, and dried to obtain a modified powder;

[0023] (3) preparing a methanol solution of 3,4-dihydroxybenzaldehyde, wherein the concentration of 3,4-dihydroxybenzaldehyde in the methanol solution is 10 g / 100 mL, and the solvent is methanol; stirring the methanol solution of 3,4-dihydroxybenzaldehyde at 50 r / min, adding p-phenylenediamine to the solution under stirring, wherein the mass ratio of the added p-phenylenediamine to the methanol solution of 3,4-dihydroxybenzaldehyde is p-phenylenediamine / methanol solution of 3,4-dihydroxybenzaldehyde=3 g / 100 mL, and continuing to stir the solution for 10 h after the addition is completed, and adding the first modified powder to the solution after the stirring is completed, wherein the solid-liquid mass ratio of the first modified powder to the solution is solid / liquid=1:20; continuing to stir the solution for 30 min after the addition is completed, and then separating the solid and liquid, and drying the solid phase to obtain the modified nano-silica.

[0024] The method for preparing the above-mentioned porcelain insulator comprises the following steps:

[0025] Step 1, weighing each raw material according to the weight portion, mixing each raw material to form a mixed powder, adding water to the mixed powder in a ball mill to obtain a slurry; the ball milling process is: the weight ratio of ball to water is ball: water: material = 1:1.2:1, the ball milling speed is 100r / min, the planetary ball mill is used, and the ball milling time is 10h;

[0026] Step 2, dewatering the slurry by filter pressing, adjusting the water content of the slurry to 25wt%, and then pressing it into an insulator blank and a test sample blank, drying the blank at 100°C for 20h, then heating it to 400°C at a heating rate of 10°C / min and calcining it for 1h, then heating it to 1200°C at a heating rate of 5°C / min and sintering it for 1h, then heating it to 1280°C at a heating rate of 2°C / min and sintering it for 2h, then cooling it to 1000°C at a cooling rate of 2°C / min and keeping it for 30min, then cooling it to 600°C at a cooling rate of 5°C / min and keeping it for 30min, then cooling it to 200°C at a cooling rate of 10°C / min, taking it out and air cooling it to room temperature to obtain the porcelain insulator and the test sample.

[0027] Example 2

[0028] A high-strength aging-resistant porcelain insulator comprises a porcelain core and an shed, wherein the shed is mounted on the outside of the porcelain core, and steel caps are bonded to both sides of the porcelain core. The raw materials of the porcelain core include: alumina, clay, potassium feldspar, zirconium oxide, modified nano silicon dioxide, titanium dioxide, bentonite and dolomite powder; the raw materials of the porcelain core are as follows by weight: 50 parts of alumina, 18 parts of clay, 13 parts of potassium feldspar, 9 parts of zirconium oxide, 22 parts of modified nano silicon dioxide, 5 parts of titanium dioxide, 8 parts of bentonite and 3 parts of dolomite powder; all raw materials are powders passing through a 400-mesh sieve; the preparation method of the modified nano silicon dioxide is as follows:

[0029] (1) In a reaction kettle, a mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol, a mixed aqueous solution of calcium nitrate and urea, and a composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol are prepared; in the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol, the concentration of hexadecyltrimethylammonium bromide is 3 g / 100 mL, the concentration of urea is 2 g / 100 mL, the concentration of ethylene glycol is 14 mL / 100 mL, and the solvent is water; In the mixed aqueous solution of calcium nitrate and urea, the concentration of calcium nitrate is 2.2 g / 100 mL, the concentration of urea is 0.9 g / 100 mL, and the solvent is water; in the composite solution of tetraethyl orthosilicate, cyclohexane, and n-pentanol, the mixing ratio of tetraethyl orthosilicate, cyclohexane, and n-pentanol is tetraethyl orthosilicate: cyclohexane: n-pentanol = 6 g: 100 mL: 4 mL; the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea, and ethylene glycol is stirred at 50 r / min, and during the stirring process, The mixed aqueous solution of calcium nitrate and urea is first added to the solution, and the solution is stirred for 30 minutes after the addition is completed. Then, the composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol is added dropwise to the solution under stirring to obtain a mixed solution, and the mixed solution is stirred for 30 minutes. The volume ratio of the mixed aqueous solution of calcium nitrate and urea and the composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol to the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol is 3:1:10: the mixed aqueous solution of calcium nitrate and urea: the composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol: the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol; then the reactor is closed, heated to 120±5°C and kept warm for 8 hours, air-cooled to room temperature after the insulation is completed, the reactor is opened, the solid-liquid separation is carried out, the solid phase is washed twice with ethanol and deionized water respectively, dried at 80°C for 20 minutes, and then calcined at 550°C for 5 hours, and air-cooled to room temperature to obtain a doped solid phase;

[0030] (2) preparing a mixed aqueous solution of magnesium chloride and ethanol, wherein the concentration of magnesium chloride in the mixed aqueous solution of magnesium chloride and ethanol is 6 g / 100 mL and the volume percentage of ethanol is 60%; the solution is kept at a constant temperature of 60±3° C. in a water bath, and the solution is stirred at a constant temperature of 50 r / min, and oleic acid is added to the solution under stirring, wherein the mass ratio of the added oleic acid to the mixed aqueous solution of magnesium chloride and ethanol is oleic acid: the mixed aqueous solution of magnesium chloride and ethanol = 2:100; after the addition is completed, the solution is stirred at a constant temperature of 60±3° C. for 30 minutes, and then the doped solid phase is added to the solution under stirring to form a suspension, and the suspension is stirred at 100° C. The doped solid phase is added to the solution to form a suspension with a solid-liquid mass ratio of solid / liquid = 1:20; after the addition is completed, the suspension is stirred at a constant temperature of 60±3°C and 50r / min for 10min, and then a sodium hydroxide solution is added dropwise to the suspension under stirring, wherein the concentration of sodium hydroxide in the sodium hydroxide solution is 1mol / L, and the volume ratio of the added volume of the sodium hydroxide solution to the suspension is sodium hydroxide solution: suspension = 1:5; after the addition is completed, the suspension is stirred at a constant temperature for 40min, air-cooled to room temperature, solid-liquid separated, the solid phase is washed twice with ethanol and deionized water, and dried to obtain a modified powder;

[0031] (3) preparing a methanol solution of 3,4-dihydroxybenzaldehyde, wherein the concentration of 3,4-dihydroxybenzaldehyde in the methanol solution is 11 g / 100 mL, and the solvent is methanol; stirring the methanol solution of 3,4-dihydroxybenzaldehyde at 50 r / min, adding p-phenylenediamine to the solution under stirring, wherein the mass ratio of the added p-phenylenediamine to the methanol solution of 3,4-dihydroxybenzaldehyde is p-phenylenediamine / methanol solution of 3,4-dihydroxybenzaldehyde=4 g / 100 mL, and continuing to stir the solution for 10 h after the addition is completed, and adding the first modified powder to the solution after the stirring is completed, wherein the solid-liquid mass ratio of the first modified powder to the solution is solid / liquid=1:20; continuing to stir the solution for 30 min after the addition is completed, and then separating the solid and liquid, and drying the solid phase to obtain the modified nano-silica.

[0032] The method for preparing the above-mentioned porcelain insulator comprises the following steps:

[0033] Step 1, weighing each raw material according to the weight portion, mixing each raw material to form a mixed powder, adding water to the mixed powder in a ball mill to obtain a slurry; the ball milling process is: the weight ratio of ball to water is ball: water: material = 1:1.2:1, the ball milling speed is 100r / min, the planetary ball mill is used, and the ball milling time is 10h;

[0034] Step 2, dewatering the slurry by filter pressing, adjusting the water content of the slurry to 25wt%, and then pressing it into an insulator blank and a test sample blank, drying the blank at 100°C for 20h, then heating it to 400°C at a heating rate of 10°C / min and calcining it for 1h, then heating it to 1200°C at a heating rate of 5°C / min and sintering it for 1h, then heating it to 1280°C at a heating rate of 2°C / min and sintering it for 2h, then cooling it to 1000°C at a cooling rate of 2°C / min and keeping it for 30min, then cooling it to 600°C at a cooling rate of 5°C / min and keeping it for 30min, then cooling it to 200°C at a cooling rate of 10°C / min, taking it out and air cooling it to room temperature to obtain the porcelain insulator and the test sample.

[0035] Example 3

[0036] A high-strength aging-resistant porcelain insulator comprises a porcelain core and an shed, wherein the shed is mounted on the outside of the porcelain core, and steel caps are bonded to both sides of the porcelain core. The raw materials of the porcelain core comprise: alumina, clay, potassium feldspar, zirconium oxide, modified nano silicon dioxide, titanium dioxide, bentonite and dolomite powder; the raw materials of the porcelain core are as follows by weight: 50 parts of alumina, 18 parts of clay, 14 parts of potassium feldspar, 9 parts of zirconium oxide, 24 parts of modified nano silicon dioxide, 7 parts of titanium dioxide, 8 parts of bentonite and 4 parts of dolomite powder; all raw materials are powders passing through a 400-mesh sieve; the preparation method of the modified nano silicon dioxide is as follows:

[0037] (1) In a reaction kettle, a mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol, a mixed aqueous solution of calcium nitrate and urea, and a composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol are prepared; in the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol, the concentration of hexadecyltrimethylammonium bromide is 4 g / 100 mL, the concentration of urea is 2 g / 100 mL, the concentration of ethylene glycol is 17 mL / 100 mL, and the solvent is water; In the mixed aqueous solution of calcium nitrate and urea, the concentration of calcium nitrate is 2.3 g / 100 mL, the concentration of urea is 0.9 g / 100 mL, and the solvent is water; in the composite solution of tetraethyl orthosilicate, cyclohexane, and n-pentanol, the mixing ratio of tetraethyl orthosilicate, cyclohexane, and n-pentanol is tetraethyl orthosilicate: cyclohexane: n-pentanol = 7 g: 100 mL: 5 mL; the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea, and ethylene glycol is stirred at 50 r / min, and during the stirring process, The mixed aqueous solution of calcium nitrate and urea is first added to the solution, and the solution is stirred for 30 minutes after the addition is completed. Then, the composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol is added dropwise to the solution under stirring to obtain a mixed solution, and the mixed solution is stirred for 30 minutes. The volume ratio of the mixed aqueous solution of calcium nitrate and urea and the composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol to the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol is 3:1:10: the mixed aqueous solution of calcium nitrate and urea: the composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol: the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol; then the reactor is closed, heated to 120±5°C and kept warm for 8 hours, air-cooled to room temperature after the insulation is completed, the reactor is opened, the solid-liquid separation is carried out, the solid phase is washed twice with ethanol and deionized water respectively, dried at 80°C for 20 minutes, and then calcined at 550°C for 5 hours, and air-cooled to room temperature to obtain a doped solid phase;

[0038] (2) preparing a mixed aqueous solution of magnesium chloride and ethanol, wherein the concentration of magnesium chloride in the mixed aqueous solution of magnesium chloride and ethanol is 6 g / 100 mL and the volume percentage of ethanol is 70%; the solution is kept at a constant temperature of 60±3° C. in a water bath, and the solution is stirred at a constant temperature of 50 r / min, and oleic acid is added to the solution under stirring, and the mass ratio of the added oleic acid to the mixed aqueous solution of magnesium chloride and ethanol is oleic acid: mixed aqueous solution of magnesium chloride and ethanol = 3:100; after the addition is completed, the solution is stirred at a constant temperature of 60±3° C. for 30 minutes, and then the doped solid phase is added to the solution under stirring to form a suspension, and The doped solid phase is added to the solution to form a suspension with a solid-liquid mass ratio of solid / liquid = 1:20; after the addition is completed, the suspension is stirred at a constant temperature of 60±3°C and 50r / min for 10min, and then a sodium hydroxide solution is added dropwise to the suspension under stirring, wherein the concentration of sodium hydroxide in the sodium hydroxide solution is 1mol / L, and the volume ratio of the added volume of the sodium hydroxide solution to the suspension is sodium hydroxide solution: suspension = 1:5; after the addition is completed, the suspension is stirred at a constant temperature for 40min, air-cooled to room temperature, solid-liquid separated, the solid phase is washed twice with ethanol and deionized water, and dried to obtain a modified powder;

[0039] (3) preparing a methanol solution of 3,4-dihydroxybenzaldehyde, wherein the concentration of 3,4-dihydroxybenzaldehyde in the methanol solution is 11 g / 100 mL, and the solvent is methanol; stirring the methanol solution of 3,4-dihydroxybenzaldehyde at 50 r / min, adding p-phenylenediamine to the solution under stirring, wherein the mass ratio of the added p-phenylenediamine to the methanol solution of 3,4-dihydroxybenzaldehyde is p-phenylenediamine / methanol solution of 3,4-dihydroxybenzaldehyde=4 g / 100 mL, and continuing to stir the solution for 10 h after the addition is completed, and adding the first modified powder to the solution after the stirring is completed, wherein the solid-liquid mass ratio of the first modified powder to the solution is solid / liquid=1:20; continuing to stir the solution for 30 min after the addition is completed, and then separating the solid and liquid, and drying the solid phase to obtain the modified nano-silica.

[0040] The method for preparing the above-mentioned porcelain insulator comprises the following steps:

[0041] Step 1, weighing each raw material according to the weight portion, mixing each raw material to form a mixed powder, adding water to the mixed powder in a ball mill to obtain a slurry; the ball milling process is: the weight ratio of ball to water is ball: water: material = 1:1.2:1, the ball milling speed is 100r / min, the planetary ball mill is used, and the ball milling time is 10h;

[0042] Step 2, dewatering the slurry by filter pressing, adjusting the water content of the slurry to 25wt%, and then pressing it into an insulator blank and a test sample blank, drying the blank at 100°C for 20h, then heating it to 400°C at a heating rate of 10°C / min and calcining it for 1h, then heating it to 1200°C at a heating rate of 5°C / min and sintering it for 1h, then heating it to 1280°C at a heating rate of 2°C / min and sintering it for 2h, then cooling it to 1000°C at a cooling rate of 2°C / min and keeping it for 30min, then cooling it to 600°C at a cooling rate of 5°C / min and keeping it for 30min, then cooling it to 200°C at a cooling rate of 10°C / min, taking it out and air cooling it to room temperature to obtain the porcelain insulator and the test sample.

[0043] Example 4

[0044] A high-strength aging-resistant porcelain insulator comprises a porcelain core and an shed, wherein the shed is mounted on the outside of the porcelain core, and steel caps are bonded to both sides of the porcelain core. The raw materials of the porcelain core comprise: alumina, clay, potassium feldspar, zirconium oxide, modified nano silicon dioxide, titanium dioxide, bentonite and dolomite powder; the raw materials of the porcelain core are as follows by weight: 50 parts of alumina, 20 parts of clay, 15 parts of potassium feldspar, 10 parts of zirconium oxide, 26 parts of modified nano silicon dioxide, 8 parts of titanium dioxide, 10 parts of bentonite and 5 parts of dolomite powder; all raw materials are powders that pass through a 400-mesh sieve; the preparation method of the modified nano silicon dioxide is as follows:

[0045] (1) In a reaction kettle, a mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol, a mixed aqueous solution of calcium nitrate and urea, and a composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol are prepared; in the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol, the concentration of hexadecyltrimethylammonium bromide is 4 g / 100 mL, the concentration of urea is 2.6 g / 100 mL, the concentration of ethylene glycol is 20 mL / 100 mL, and the solvent is water. ; In the mixed aqueous solution of calcium nitrate and urea, the concentration of calcium nitrate is 2.5g / 100mL, the concentration of urea is 1g / 100mL, and the solvent is water; in the composite solution of tetraethyl orthosilicate, cyclohexane, and n-pentanol, the mixing ratio of tetraethyl orthosilicate, cyclohexane, and n-pentanol is tetraethyl orthosilicate: cyclohexane: n-pentanol = 7g: 100mL: 5mL; the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea, and ethylene glycol is stirred at 50r / min, and during the stirring process, The mixed aqueous solution of calcium nitrate and urea is first added to the solution, and the solution is stirred for 30 minutes after the addition is completed. Then, the composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol is added dropwise to the solution under stirring to obtain a mixed solution, and the mixed solution is stirred for 30 minutes. The volume ratio of the mixed aqueous solution of calcium nitrate and urea and the composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol to the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol is 3:1:10: the mixed aqueous solution of calcium nitrate and urea: the composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol: the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol; then the reactor is closed, heated to 120±5°C and kept warm for 8 hours, air-cooled to room temperature after the insulation is completed, the reactor is opened, the solid-liquid separation is carried out, the solid phase is washed twice with ethanol and deionized water respectively, dried at 80°C for 20 minutes, and then calcined at 550°C for 5 hours, and air-cooled to room temperature to obtain a doped solid phase;

[0046] (2) preparing a mixed aqueous solution of magnesium chloride and ethanol, wherein the concentration of magnesium chloride in the mixed aqueous solution of magnesium chloride and ethanol is 7 g / 100 mL and the volume percentage of ethanol is 70%; placing the solution in a water bath at a constant temperature of 60±3° C., stirring the solution at a constant temperature of 50 r / min, adding oleic acid to the solution under stirring, wherein the mass ratio of the added oleic acid to the mixed aqueous solution of magnesium chloride and ethanol is oleic acid: the mixed aqueous solution of magnesium chloride and ethanol = 3:100; after the addition is completed, continuing to stir the solution at a constant temperature of 60±3° C. for 30 min, then adding the doped solid phase to the solution under stirring to form a suspension, and The doped solid phase is added to the solution to form a suspension with a solid-liquid mass ratio of solid / liquid = 1:20; after the addition is completed, the suspension is stirred at a constant temperature of 60±3°C and 50r / min for 10min, and then a sodium hydroxide solution is added dropwise to the suspension under stirring, wherein the concentration of sodium hydroxide in the sodium hydroxide solution is 1mol / L, and the volume ratio of the added volume of the sodium hydroxide solution to the suspension is sodium hydroxide solution: suspension = 1:5; after the addition is completed, the suspension is stirred at a constant temperature for 40min, air-cooled to room temperature, solid-liquid separated, the solid phase is washed twice with ethanol and deionized water, and dried to obtain a modified powder;

[0047] (3) preparing a methanol solution of 3,4-dihydroxybenzaldehyde, wherein the concentration of 3,4-dihydroxybenzaldehyde in the methanol solution is 12 g / 100 mL, and the solvent is methanol; stirring the methanol solution of 3,4-dihydroxybenzaldehyde at 50 r / min, adding p-phenylenediamine to the solution under stirring, wherein the mass ratio of the added p-phenylenediamine to the methanol solution of 3,4-dihydroxybenzaldehyde is p-phenylenediamine / methanol solution of 3,4-dihydroxybenzaldehyde=5 g / 100 mL, and continuing to stir the solution for 10 h after the addition is completed, and adding the first modified powder to the solution after the stirring is completed, wherein the solid-liquid mass ratio of the first modified powder to the solution is solid / liquid=1:20; and continuing to stir the solution for 30 min after the addition is completed, and then separating the solid and liquid, and drying the solid phase to obtain the modified nano-silica.

[0048] The method for preparing the above-mentioned porcelain insulator comprises the following steps:

[0049] Step 1, weighing each raw material according to the weight portion, mixing each raw material to form a mixed powder, adding water to the mixed powder in a ball mill to obtain a slurry; the ball milling process is: the weight ratio of ball to water is ball: water: material = 1:1.2:1, the ball milling speed is 100r / min, the planetary ball mill is used, and the ball milling time is 10h;

[0050] Step 2, dewatering the slurry by filter pressing, adjusting the water content of the slurry to 25wt%, and then pressing it into an insulator blank and a test sample blank, drying the blank at 100°C for 20h, then heating it to 400°C at a heating rate of 10°C / min and calcining it for 1h, then heating it to 1200°C at a heating rate of 5°C / min and sintering it for 1h, then heating it to 1280°C at a heating rate of 2°C / min and sintering it for 2h, then cooling it to 1000°C at a cooling rate of 2°C / min and keeping it for 30min, then cooling it to 600°C at a cooling rate of 5°C / min and keeping it for 30min, then cooling it to 200°C at a cooling rate of 10°C / min, taking it out and air cooling it to room temperature to obtain the porcelain insulator and the test sample.

[0051] Comparative Example 1

[0052] A comparative porcelain insulator comprises a porcelain core and an shed, wherein the shed is mounted on the outside of the porcelain core, and steel caps are bonded to both sides of the porcelain core. The raw materials of the porcelain core include: alumina, clay, potassium feldspar, zirconium oxide, modified nano-silicon dioxide, titanium dioxide, bentonite and dolomite powder; the raw materials of the porcelain core are calculated by weight as follows: 50 parts of alumina, 18 parts of clay, 13 parts of potassium feldspar, 9 parts of zirconium oxide, 22 parts of modified nano-silicon dioxide, 5 parts of titanium dioxide, 8 parts of bentonite and 3 parts of dolomite powder; all raw materials are powders passing through a 400-mesh sieve; the preparation method of the modified nano-silicon dioxide is as follows:

[0053] (1) In a reaction kettle, a mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol, an aqueous solution of urea, and a composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol are prepared; in the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol, the concentration of hexadecyltrimethylammonium bromide is 3 g / 100 mL, the concentration of urea is 2 g / 100 mL, the concentration of ethylene glycol is 14 mL / 100 mL, and the solvent is water; in the aqueous solution of urea, the concentration of urea is 0.9 g / 100 mL, and the solvent is water; in the composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol, the mixing ratio of tetraethyl orthosilicate, cyclohexane and n-pentanol is tetraethyl orthosilicate: cyclohexane: n-pentanol = 6 g: 100 mL: 4 mL; the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol is stirred at 50 r / min, and during the stirring process, the urea is first added to the solution. The aqueous solution of tetraethyl orthosilicate, cyclohexane, and n-pentanol was added, and the solution was stirred for 30 minutes after the addition was completed. Then, the composite solution of tetraethyl orthosilicate, cyclohexane, and n-pentanol was added dropwise to the solution under stirring to obtain a mixed solution. The mixed solution was stirred for 30 minutes, and the volume ratio of the aqueous solution of urea and the composite solution of tetraethyl orthosilicate, cyclohexane, and n-pentanol to the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea, and ethylene glycol was 3:1:10; then the reactor was closed, heated to 120±5°C and kept warm for 8 hours, and air-cooled to room temperature after the insulation was completed. The reactor was opened, the solid-liquid separation was carried out, the solid phase was washed twice with ethanol and deionized water, dried at 80°C for 20 minutes, and then calcined at 550°C for 5 hours, and air-cooled to room temperature to obtain the solid phase product powder of this comparative example;

[0054] (2) preparing a mixed aqueous solution of magnesium chloride and ethanol, wherein the concentration of magnesium chloride is 6 g / 100 mL and the volume percentage of ethanol is 60%; the solution is kept at a constant temperature of 60±3° C. in a water bath, and the solution is stirred at a constant temperature of 50 r / min, and oleic acid is added to the solution under stirring, wherein the mass ratio of the added oleic acid to the mixed aqueous solution of magnesium chloride and ethanol is oleic acid: the mixed aqueous solution of magnesium chloride and ethanol = 2:100; after the addition is completed, the solution is stirred at a constant temperature of 60±3° C. for 30 minutes, and then the solid phase product powder is added to the solution under stirring to form a suspension, and the mixture is stirred at 40° C. for 30 minutes. The solid phase product powder is added to the solution to form a suspension with a solid-liquid mass ratio of solid / liquid = 1:20; after the addition is completed, the suspension is stirred at a constant temperature of 60±3°C and 50r / min for 10min, and then a sodium hydroxide solution is added dropwise to the suspension under stirring, wherein the concentration of sodium hydroxide in the sodium hydroxide solution is 1mol / L, and the volume ratio of the added volume of the sodium hydroxide solution to the suspension is sodium hydroxide solution: suspension = 1:5; after the addition is completed, the suspension is stirred at a constant temperature for 40min, air-cooled to room temperature, solid-liquid separated, the solid phase is washed twice with ethanol and deionized water, and dried to obtain a primary modified powder;

[0055] (3) preparing a methanol solution of 3,4-dihydroxybenzaldehyde, wherein the concentration of 3,4-dihydroxybenzaldehyde in the methanol solution is 11 g / 100 mL, and the solvent is methanol; stirring the methanol solution of 3,4-dihydroxybenzaldehyde at 50 r / min, adding p-phenylenediamine to the solution under stirring, wherein the mass ratio of the added p-phenylenediamine to the methanol solution of 3,4-dihydroxybenzaldehyde is p-phenylenediamine / methanol solution of 3,4-dihydroxybenzaldehyde=4 g / 100 mL, and continuing to stir the solution for 10 h after the addition is completed, and adding the first modified powder to the solution after the stirring is completed, wherein the solid-liquid mass ratio of the first modified powder to the solution is solid / liquid=1:20; continuing to stir the solution for 30 min after the addition is completed, and then separating the solid and liquid, and drying the solid phase to obtain the modified nano-silica described in this comparative example.

[0056] The method for preparing the above-mentioned porcelain insulator comprises the following steps:

[0057] Step 1, weighing each raw material according to the weight portion, mixing each raw material to form a mixed powder, adding water to the mixed powder in a ball mill to obtain a slurry; the ball milling process is: the weight ratio of ball to water is ball: water: material = 1:1.2:1, the ball milling speed is 100r / min, the planetary ball mill is used, and the ball milling time is 10h;

[0058] Step 2, dewatering the slurry by filter pressing, adjusting the water content of the slurry to 25wt%, and then pressing it into an insulator blank and a test sample blank, drying the blank at 100°C for 20h, then heating it to 400°C at a heating rate of 10°C / min and calcining it for 1h, then heating it to 1200°C at a heating rate of 5°C / min and sintering it for 1h, then heating it to 1280°C at a heating rate of 2°C / min and sintering it for 2h, then cooling it to 1000°C at a cooling rate of 2°C / min and keeping it warm for 30min, then cooling it to 600°C at a cooling rate of 5°C / min and keeping it warm for 30min, then cooling it to 200°C at a cooling rate of 10°C / min, taking it out and air cooling it to room temperature, and obtaining the porcelain insulator and the test sample of this comparative example.

[0059] Comparative Example 2

[0060] A comparative porcelain insulator comprises a porcelain core and an shed, wherein the shed is mounted on the outside of the porcelain core, and steel caps are bonded to both sides of the porcelain core. The raw materials of the porcelain core include: alumina, clay, potassium feldspar, zirconium oxide, modified nano-silicon dioxide, titanium dioxide, bentonite and dolomite powder; the raw materials of the porcelain core are calculated by weight as follows: 50 parts of alumina, 18 parts of clay, 13 parts of potassium feldspar, 9 parts of zirconium oxide, 22 parts of modified nano-silicon dioxide, 5 parts of titanium dioxide, 8 parts of bentonite and 3 parts of dolomite powder; all raw materials are powders passing through a 400-mesh sieve; the preparation method of the modified nano-silicon dioxide is as follows:

[0061] (1) In a reaction kettle, a mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol, a mixed aqueous solution of calcium nitrate and urea, and a composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol are prepared; in the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol, the concentration of hexadecyltrimethylammonium bromide is 3 g / 100 mL, the concentration of urea is 2 g / 100 mL, the concentration of ethylene glycol is 14 mL / 100 mL, and the solvent is water; In the mixed aqueous solution of calcium nitrate and urea, the concentration of calcium nitrate is 2.2 g / 100 mL, the concentration of urea is 0.9 g / 100 mL, and the solvent is water; in the composite solution of tetraethyl orthosilicate, cyclohexane, and n-pentanol, the mixing ratio of tetraethyl orthosilicate, cyclohexane, and n-pentanol is tetraethyl orthosilicate: cyclohexane: n-pentanol = 6 g: 100 mL: 4 mL; the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea, and ethylene glycol is stirred at 50 r / min, and during the stirring process, The mixed aqueous solution of calcium nitrate and urea is first added to the solution, and the solution is stirred for 30 minutes after the addition is completed. Then, the composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol is added dropwise to the solution under stirring to obtain a mixed solution, and the mixed solution is stirred for 30 minutes. The volume ratio of the mixed aqueous solution of calcium nitrate and urea and the composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol to the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol is 3:1:10: the mixed aqueous solution of calcium nitrate and urea: the composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol: the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol; then the reactor is closed, heated to 120±5°C and kept warm for 8 hours, air-cooled to room temperature after the insulation is completed, the reactor is opened, the solid-liquid separation is carried out, the solid phase is washed twice with ethanol and deionized water respectively, dried at 80°C for 20 minutes, and then calcined at 550°C for 5 hours, and air-cooled to room temperature to obtain a doped solid phase;

[0062] (2) preparing a methanol solution of 3,4-dihydroxybenzaldehyde, wherein the concentration of 3,4-dihydroxybenzaldehyde in the methanol solution is 11 g / 100 mL, and the solvent is methanol; stirring the methanol solution of 3,4-dihydroxybenzaldehyde at 50 r / min, adding p-phenylenediamine to the solution under stirring, wherein the mass ratio of the added p-phenylenediamine to the methanol solution of 3,4-dihydroxybenzaldehyde is p-phenylenediamine / methanol solution of 3,4-dihydroxybenzaldehyde=4 g / 100 mL, and continuing to stir the solution for 10 h after the addition is completed, and adding the doped solid phase to the solution, wherein the solid-liquid mass ratio of the doped solid phase added to the solution is solid / liquid=1:20; continuing to stir the solution for 30 min after the addition is completed, and then separating the solid and liquid, and drying the solid phase to obtain the modified nano-silica described in this comparative example.

[0063] The method for preparing the above-mentioned porcelain insulator comprises the following steps:

[0064] Step 1, weighing each raw material according to the weight portion, mixing each raw material to form a mixed powder, adding water to the mixed powder in a ball mill to obtain a slurry; the ball milling process is: the weight ratio of ball to water is ball: water: material = 1:1.2:1, the ball milling speed is 100r / min, the planetary ball mill is used, and the ball milling time is 10h;

[0065] Step 2, dewatering the slurry by filter pressing, adjusting the water content of the slurry to 25wt%, and then pressing it into an insulator blank and a test sample blank, drying the blank at 100°C for 20h, then heating it to 400°C at a heating rate of 10°C / min and calcining it for 1h, then heating it to 1200°C at a heating rate of 5°C / min and sintering it for 1h, then heating it to 1280°C at a heating rate of 2°C / min and sintering it for 2h, then cooling it to 1000°C at a cooling rate of 2°C / min and keeping it warm for 30min, then cooling it to 600°C at a cooling rate of 5°C / min and keeping it warm for 30min, then cooling it to 200°C at a cooling rate of 10°C / min, taking it out and air cooling it to room temperature, and obtaining the porcelain insulator and the test sample of this comparative example.

[0066] Comparative Example 3

[0067] A comparative porcelain insulator comprises a porcelain core and an shed, wherein the shed is mounted on the outside of the porcelain core, and steel caps are bonded to both sides of the porcelain core. The raw materials of the porcelain core include: alumina, clay, potassium feldspar, zirconium oxide, modified nano-silicon dioxide, titanium dioxide, bentonite and dolomite powder; the raw materials of the porcelain core are calculated by weight as follows: 50 parts of alumina, 18 parts of clay, 13 parts of potassium feldspar, 9 parts of zirconium oxide, 22 parts of modified nano-silicon dioxide, 5 parts of titanium dioxide, 8 parts of bentonite and 3 parts of dolomite powder; all raw materials are powders passing through a 400-mesh sieve; the preparation method of the modified nano-silicon dioxide is as follows:

[0068] (1) In a reaction kettle, a mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol, a mixed aqueous solution of calcium nitrate and urea, and a composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol are prepared; in the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol, the concentration of hexadecyltrimethylammonium bromide is 3 g / 100 mL, the concentration of urea is 2 g / 100 mL, the concentration of ethylene glycol is 14 mL / 100 mL, and the solvent is water; In the mixed aqueous solution of calcium nitrate and urea, the concentration of calcium nitrate is 2.2 g / 100 mL, the concentration of urea is 0.9 g / 100 mL, and the solvent is water; in the composite solution of tetraethyl orthosilicate, cyclohexane, and n-pentanol, the mixing ratio of tetraethyl orthosilicate, cyclohexane, and n-pentanol is tetraethyl orthosilicate: cyclohexane: n-pentanol = 6 g: 100 mL: 4 mL; the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea, and ethylene glycol is stirred at 50 r / min, and during the stirring process, The mixed aqueous solution of calcium nitrate and urea is first added to the solution, and the solution is stirred for 30 minutes after the addition is completed. Then, the composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol is added dropwise to the solution under stirring to obtain a mixed solution, and the mixed solution is stirred for 30 minutes. The volume ratio of the mixed aqueous solution of calcium nitrate and urea and the composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol to the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol is 3:1:10: the mixed aqueous solution of calcium nitrate and urea: the composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol: the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol; then the reactor is closed, heated to 120±5°C and kept warm for 8 hours, air-cooled to room temperature after the insulation is completed, the reactor is opened, the solid-liquid separation is carried out, the solid phase is washed twice with ethanol and deionized water respectively, dried at 80°C for 20 minutes, and then calcined at 550°C for 5 hours, and air-cooled to room temperature to obtain a doped solid phase;

[0069] (2) preparing a mixed aqueous solution of magnesium chloride and ethanol, wherein the concentration of magnesium chloride is 6 g / 100 mL and the volume percentage of ethanol is 60%; placing the solution in a water bath at a constant temperature of 60±3° C., stirring the solution at a constant temperature of 50 r / min, adding oleic acid to the solution under stirring, wherein the mass ratio of the added oleic acid to the mixed aqueous solution of magnesium chloride and ethanol is oleic acid: the mixed aqueous solution of magnesium chloride and ethanol = 2:100; after the addition is completed, the solution is stirred at a constant temperature of 60±3° C. for 30 min, and then the doped solid phase is added to the solution under stirring to form a suspension, and the doped solid phase is added to the solution. The solid-liquid mass ratio of the suspension formed by the impure solid phase is solid / liquid=1:20; after the addition is completed, the suspension is stirred at a constant temperature of 60±3°C and 50r / min for 10min, and then a sodium hydroxide solution is added dropwise to the suspension under stirring, wherein the concentration of sodium hydroxide in the sodium hydroxide solution is 1mol / L, and the volume ratio of the added volume of the sodium hydroxide solution to the suspension is sodium hydroxide solution: suspension=1:5; after the addition is completed, the suspension is stirred at a constant temperature for 40min, air-cooled to room temperature, solid-liquid separated, the solid phase is washed twice with ethanol and deionized water respectively, and dried to obtain a modified powder as the modified nano-silica of this comparative example.

[0070] The method for preparing the above-mentioned porcelain insulator comprises the following steps:

[0071] Step 1, weighing each raw material according to the weight portion, mixing each raw material to form a mixed powder, adding water to the mixed powder in a ball mill to obtain a slurry; the ball milling process is: the weight ratio of ball to water is ball: water: material = 1:1.2:1, the ball milling speed is 100r / min, the planetary ball mill is used, and the ball milling time is 10h;

[0072] Step 2, dewatering the slurry by filter pressing, adjusting the water content of the slurry to 25wt%, and then pressing it into an insulator blank and a test sample blank, drying the blank at 100°C for 20h, then heating it to 400°C at a heating rate of 10°C / min and calcining it for 1h, then heating it to 1200°C at a heating rate of 5°C / min and sintering it for 1h, then heating it to 1280°C at a heating rate of 2°C / min and sintering it for 2h, then cooling it to 1000°C at a cooling rate of 2°C / min and keeping it warm for 30min, then cooling it to 600°C at a cooling rate of 5°C / min and keeping it warm for 30min, then cooling it to 200°C at a cooling rate of 10°C / min, taking it out and air cooling it to room temperature, and obtaining the porcelain insulator and the test sample of this comparative example.

[0073] Example 5

[0074] The bending strength of the test samples prepared by the methods described in the above embodiments and comparative examples was tested according to the requirements of standard GB / T 4741-1999, and the loading speed was set to 20N / s; the breakdown voltage of the test samples prepared by the methods described in the above embodiments and comparative examples was tested using an impulse voltage generator to simulate the lightning strike effect; each group of test samples was repeatedly frozen and thawed 30 times at -50°C to 40°C, first the sample was placed in a box at a constant temperature of -50°C and allowed to stand for 20 minutes, then taken out and allowed to stand in the air for 10 minutes, then the sample was placed in a box at a constant temperature of 40°C and allowed to stand for 20 minutes, and after the standing was completed, it was taken out and allowed to stand in the air for 10 minutes, that is, one freeze-thaw process was completed, and whether there were cracks on the surface of the sample after 30 freeze-thaw cycles, the results are shown in Table 1.

[0075] Table 1

[0076] Experimental Group Bending strength / MPa Breakdown voltage / kV Is there any crack after 30 freeze-thaw cycles? Example 1 422 144 No cracks Example 2 431 149 No cracks Example 3 428 146 No cracks Example 4 425 142 No cracks Comparative Example 1 384 131 A few cracks Comparative Example 2 370 127 A few cracks Comparative Example 3 377 124 A few cracks

[0077] As shown in Table 1, the porcelain core for porcelain insulators prepared by the method of the present invention has a high flexural strength breakdown voltage, improves the safety and durability of the insulator, and reduces the failure rate of the porcelain insulator. At the same time, it will not crack after repeated freezing and thawing, has good aging resistance, and is suitable for use in areas with large temperature changes.

[0078] The technical solution provided by the present invention is introduced in detail above. For those skilled in the art, according to the concept of the embodiments of the present invention, there may be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A high-strength, aging-resistant porcelain insulator, comprising a porcelain core and a shed skirt, wherein the shed skirt is sleeved on the outside of the porcelain core, and steel caps are bonded on both sides of the porcelain core, characterized in that: The raw materials of the porcelain core include: alumina, clay, potassium feldspar, zirconium oxide, modified nano silicon dioxide, titanium dioxide, bentonite and dolomite powder; the raw materials of the porcelain core are calculated by weight as follows: 50 parts of alumina, 16-20 parts of clay, 12-15 parts of potassium feldspar, 8-10 parts of zirconium oxide, 20-26 parts of modified nano silicon dioxide, 3-8 parts of titanium dioxide, 6-10 parts of bentonite, and 2-5 parts of dolomite powder; all raw materials are powders that pass through a 400-mesh sieve; the preparation method of the modified nano silicon dioxide is: (1) in a reaction kettle, a mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol, a mixed aqueous solution of calcium nitrate and urea, and a composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol are prepared; the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol is stirred, and the mixed aqueous solution of calcium nitrate and urea is first added to the solution during the stirring process, and the solution is stirred for more than 30 minutes after the addition is completed, and then the composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol is added dropwise to the solution under stirring to obtain a mixed solution, and the mixed solution is stirred for more than 30 minutes, and then the reaction kettle is closed, heated to 120±5° C. and kept warm for more than 8 hours, and then air-cooled to room temperature after the insulation is completed, and the reaction kettle is opened for solid-liquid separation, and the solid phase is washed twice with ethanol and deionized water, respectively, and dried at 80° C. for more than 20 minutes, and then calcined at 550° C. for 5-6 hours, and air-cooled to room temperature to obtain a doped solid phase; (2) preparing a mixed aqueous solution of magnesium chloride and ethanol, keeping the solution constant temperature at 60±3° C. in a water bath, stirring the solution at the constant temperature, adding oleic acid to the solution under stirring, and continuing to stir the solution at a constant temperature of 60±3° C. for more than 30 minutes after the addition is completed, then adding the doped solid phase to the solution under stirring to form a suspension, and continuing to stir the suspension at a constant temperature of 60±3° C. for more than 10 minutes after the addition is completed, and then dropping sodium hydroxide solution into the suspension under stirring, and continuing to stir the suspension at a constant temperature for more than 40 minutes after the addition is completed, air cooling to room temperature, solid-liquid separation, washing the solid phase with ethanol and deionized water twice each, and drying to obtain a primary modified powder; (3) preparing a methanol solution of 3,4-dihydroxybenzaldehyde, stirring the methanol solution of 3,4-dihydroxybenzaldehyde, adding p-phenylenediamine to the solution under stirring, continuing to stir the solution for more than 10 hours after the addition is completed, adding the primary modified powder to the solution after the addition is completed, continuing to stir the solution for more than 30 minutes after the addition is completed, then separating the solid and liquid, and drying the solid phase to obtain the modified nano-silica.

2. A high-strength, aging-resistant porcelain insulator according to claim 1, characterized in that: In the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol, the concentration of hexadecyltrimethylammonium bromide is 3-4 g / 100 mL, the concentration of urea is 1.6-2.6 g / 100 mL, the concentration of ethylene glycol is 10-20 mL / 100 mL, and the solvent is water; in the mixed aqueous solution of calcium nitrate and urea, the concentration of calcium nitrate is 2.0-2.5 g / 100 mL, the concentration of urea is 0.8-1 g / 100 mL, and the solvent is water; in the composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol, the mixing ratio of tetraethyl orthosilicate, cyclohexane and n-pentanol is tetraethyl orthosilicate: cyclohexane: n-pentanol = 6-7 g: 100 mL: 4-5 mL.

3. A high-strength, aging-resistant porcelain insulator according to claim 1, characterized in that: The volume ratio of the mixed aqueous solution of calcium nitrate and urea and the composite solution of tetraethyl orthosilicate, cyclohexane and n-pentanol to the mixed aqueous solution of hexadecyltrimethylammonium bromide, urea and ethylene glycol is 3:1:

10.

4. The high-strength aging-resistant porcelain insulator according to claim 1, characterized in that: In the step (2), in the mixed aqueous solution of magnesium chloride and ethanol, the concentration of magnesium chloride is 5-7 g / 100 mL, and the volume percentage of ethanol is 60%-70%; the mass ratio of the added mass of oleic acid to the mixed aqueous solution of magnesium chloride and ethanol is oleic acid: mixed aqueous solution of magnesium chloride and ethanol = 2-3:100; the solid-liquid mass ratio of adding the doped solid phase to the solution to form a suspension is solid / liquid = 1:20; the concentration of sodium hydroxide in the sodium hydroxide solution is 1 mol / L, and the volume ratio of the added volume of the sodium hydroxide solution to the suspension is sodium hydroxide solution: suspension = 1:

5.

5. The high-strength aging-resistant porcelain insulator according to claim 1, characterized in that: In the step (3), in the methanol solution of 3,4-dihydroxybenzaldehyde, the concentration of 3,4-dihydroxybenzaldehyde is 10-12 g / 100 mL, and the solvent is methanol; the amount ratio of the added mass of p-phenylenediamine to the methanol solution of 3,4-dihydroxybenzaldehyde is p-phenylenediamine / methanol solution of 3,4-dihydroxybenzaldehyde=3-5 g / 100 mL, and the solid-liquid mass ratio of the primary modified powder added to the solution is solid / liquid=1:

20.

6. The method for preparing a porcelain insulator according to any one of claims 1 to 5, characterized in that: The following steps are included: Step 1, weighing the raw materials according to the weight proportions, mixing the raw materials to form a mixed powder, and adding water to the mixed powder in a ball mill to obtain a slurry; Step 2: Dehydrate the slurry by filter pressing, adjust the water content of the slurry to 25wt%, and then press it into an insulator blank. The blank is dried at 100°C for 20h, then heated to 400°C at a heating rate of 10°C / min and calcined for 1h, then heated to 1200°C at a heating rate of 5°C / min and sintered for 1h, then heated to 1280°C at a heating rate of 2°C / min and sintered for 2h, then cooled to 1000°C at a cooling rate of 2°C / min and kept warm for 30min, then cooled to 600°C at a cooling rate of 5°C / min and kept warm for 30min, then cooled to 200°C at a cooling rate of 10°C / min, taken out and air-cooled to room temperature to obtain the porcelain insulator.

7. The method for preparing a porcelain insulator according to claim 6, characterized in that: The ball milling process is as follows: the weight ratio of ball to water is ball: water: material = 1:1.2:1, the ball milling speed is 100 r / min, the planetary ball mill is used, and the ball milling time is 10 h.

Citation Information

Patent Citations

  • Electric porcelain insulator and preparation method thereof

    CN108101526A

  • High-strength aging-resistant porcelain insulator and preparation method thereof

    CN110845224A

  • Manufacturing and processing technology for electric stay insulator

    CN113979733A

  • Colored glaze for porcelain insulator and preparation method thereof

    CN114804634A

  • High-voltage line column type porcelain insulator

    CN115677329A