A TiOx-coated vanadate photocatalyst and preparation method thereof
By loading precious metals on the surface of the vanadate and forming a TiOx-coated vanadate photocatalyst with amorphous titanium oxide coating, the problem of hydrogen-oxygen recombination reaction in the process of photocatalytic decomposition of water hydrogen production is solved, and efficiency and catalyst are improved The service life of the product reduces production costs.
Patent Information
- Application Number
- CN202310754078.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-25
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-06-25
AI Technical Summary
During the photocatalytic complete decomposition of water hydrogen production, the catalyst easily induces the reverse reaction of hydrogen and oxygen to recombination into water, which reduces the efficiency. In addition, the metal/Cr2O3 catalyst of the existing core-shell structure needs to be replaced regularly after long-term use, which increases Production cost.
The photocatalyst coated with vanadate is adopted to suppress the occurrence of hydrogen and oxygen recombination reaction and improve the catalyst activity and efficiency by loading precious metals on the surface of vanadate and forming a uniform amorphous titanium oxide coating layer.
It effectively reduces the occurrence of hydrogen and oxygen composite reaction on the surface of the catalyst, improves the efficiency of photocatalytic decomposition of water to produce hydrogen, extends the service life of the catalyst, and reduces production costs.
Smart Images

Figure CN116983981B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solar hydrogen production and catalysis, and particularly relates to a TiOx-coated vanadate photocatalyst and a preparation method thereof. Background Art
[0002] Using renewable energy to prepare fuel is an important way to solve the energy crisis and environmental pollution. Due to the environmental friendliness of solar energy, the cheap and easy availability of raw water, and the wide application of hydrogen in industry, solar water decomposition to produce hydrogen has received widespread attention in recent years.
[0003] Among many technical routes, solar photocatalytic hydrogen production realizes the one-step conversion from solar energy to hydrogen energy, and has the advantages of simple equipment and easy scale-up. When a photocatalyst loaded with precious metals Pt or Rh is added to pure water, hydrogen and oxygen with a stoichiometric ratio of 2:1 can be simultaneously produced under light. However, since light excitation, carrier separation, and hydrogen and oxygen evolution reactions occur simultaneously on micro-nano semiconductor particles, the realization of this process places high demands on photocatalysts. Summary of the invention
[0004] The present invention is based on the inventor's discovery and understanding of the following facts and problems:
[0005] In the process of photocatalytic decomposition of water to produce hydrogen, the catalyst will induce the reverse reaction of catalytic hydrogen and oxygen to recombine into water while catalyzing the production of hydrogen, which seriously reduces the efficiency of photocatalytic decomposition of water to produce hydrogen in the suspension system.
[0006] The most typical method to inhibit the hydrogen-oxygen recombination reaction is to use a core-shell metal / Cr2O3 catalyst. For example, it has been reported that Rh / Cr2O3 catalysts are supported on a variety of semiconductors to achieve photocatalytic water splitting reactions. The Cr2O3 layer is only a few nanometers thick and is usually coated by photodeposition. Because the active site of the hydrogen-oxygen recombination reaction is not in the Cr2O3 layer but on the surface of the metal Rh, considering the different radii of hydrogen and oxygen molecules, the Cr2O3 nanolayer can allow H2 gas to penetrate to the outer surface, but the oxygen produced by water oxidation cannot penetrate into the interior of the Cr2O3 nanolayer, preventing O2 from contacting the Rh core surface and inhibiting the reverse reaction of hydrogen and oxygen on the Rh catalyst surface to recombine into water. The activity of photocatalytic water splitting can be restored to a certain extent by supporting Rh / Cr2O3 catalysts on the surface of the photocatalyst, but the Cr2O3 nanolayer will be partially lost in the long-term photocatalytic reaction. After long-term use, the inhibitory effect on the hydrogen-oxygen recombination reaction will be reduced, and the catalyst needs to be replaced regularly, resulting in an increase in production costs.
[0007] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, an embodiment of the present invention provides a TiOx The photocatalyst coated with vanadate forms a uniform amorphous titanium oxide coating layer on the surface of the photocatalyst, which can effectively inhibit the occurrence of hydrogen-oxygen recombination reaction on the surface of the co-catalyst and improve the efficiency of photocatalytic water decomposition to produce hydrogen.
[0008] TiO in the embodiment of the present invention x A photocatalyst coated with vanadate, the photocatalyst comprising vanadate and TiO x The coating layer, the surface of the vanadate is loaded with precious metals, the TiO x The coating layer covers the surfaces of the vanadate and the noble metal.
[0009] TiO in the embodiment of the present invention x The advantages and technical effects brought by the vanadate-coated photocatalyst are as follows: 1. In the embodiment of the present invention, precious metals are loaded on the surface of the vanadate, which can effectively reduce the recombination probability of electrons and holes and improve the activity of the catalyst; 2. In the implementation of the present invention, a uniform titanium oxide coating layer is formed on the surface of the photocatalyst, which can effectively inhibit the occurrence of hydrogen-oxygen recombination reaction on the surface of the co-catalyst and improve the efficiency of photocatalytic water decomposition to produce hydrogen.
[0010] In some embodiments, the vanadate is bismuth yttrium vanadate, whose chemical formula is Bi x Y 1-x VO4, of which 0.1 <x<0.9。
[0011] In some embodiments, the noble metal includes at least one of gold, palladium, platinum or rhodium. Preferably, the loading amount of the noble metal is 0.1-1 wt %, based on the total mass of the photocatalyst.
[0012] In some embodiments, the TiO x The thickness of the layer is 1 to 6 nm. Preferably, the loading amount of Ti is 1 to 10 wt.%, based on the total mass of the photocatalyst.
[0013] The embodiment of the present invention also provides a TiO x The preparation method of the photocatalyst coated with vanadate comprises the following steps:
[0014] (1) dispersing vanadate in water, adding a noble metal salt solution, and irradiating with ultraviolet light under a vacuum environment to obtain a first suspension;
[0015] (2) adding a titanium peroxide solution to the first suspension obtained in step (1), and irradiating the suspension with ultraviolet light under a vacuum environment to obtain a second suspension;
[0016] (3) filtering, washing and drying the second suspension obtained in step (2) to obtain TiO xEncapsulated vanadate photocatalysts.
[0017] TiO in the embodiment of the present invention x The advantages and technical effects brought by the preparation method of the vanadate-coated photocatalyst are as follows: 1. The method of the embodiment of the present invention loads the noble metal promoter on the surface of the catalyst by ultraviolet irradiation under a vacuum environment, so that the noble metal atoms can be selectively anchored on the catalytic sites or electron aggregation areas on the surface of the photocatalyst, thereby reducing the migration distance of the photogenerated electrons; 2. The method of the embodiment of the present invention uniformly coats the surface of the vanadate with amorphous TiO by photoreduction of soluble titanium peroxide. x , the formed TiO x It can effectively inhibit the occurrence of hydrogen-oxygen recombination reaction on the catalyst surface and improve the efficiency of photocatalytic water decomposition to produce hydrogen; 3. The method of the embodiment of the present invention has a simple process, cheap raw materials, and does not involve complex processes such as chemical vapor deposition, physical vapor deposition and atomic deposition, which is convenient for promotion and application in industrial production.
[0018] In some embodiments, in step (1), the noble metal salt includes at least one of chloroauric acid, palladium trichloride, chloroplatinic acid and rhodium trichloride;
[0019] And / or, in the steps (1) and / or (2), the pressure of the vacuum environment is 0.1-1 KPa.
[0020] In some embodiments, in step (1) and / or (2), the wavelength of the ultraviolet light source is 200-400 nm, and the light intensity is 10-100 mW / cm 2 , the irradiation time is 1 to 3 hours.
[0021] In some embodiments, in step (1), the vanadate photocatalyst is tetragonal zircon phase bismuth yttrium vanadate, and its preparation method comprises the following steps:
[0022] A. dissolving bismuth salt, yttrium salt and vanadium salt in nitric acid solution, adding ammonia water to adjust the pH, and reacting to obtain a precipitate;
[0023] B. subjecting the precipitate obtained in step A to static aging, solid-liquid separation, washing and drying to obtain a solid powder;
[0024] C. calcining the solid powder obtained in step B to obtain tetragonal zircon phase bismuth yttrium vanadate.
[0025] In some embodiments, in step A, the molar ratio of the bismuth salt to the yttrium salt is (0.1-10):1, and the molar ratio of the total amount of the bismuth salt and the yttrium salt to the vanadium salt is (0.1-10):1; and / or, the pH is adjusted to 4-12;
[0026] And / or, in the step C, the calcination temperature is 400-1000° C., and the calcination time is 2-12 hours.
[0027] In some embodiments, in step (2), the preparation process of the titanium peroxide solution includes: adding a titanium salt to a mixed solution of water and alcohol to react to obtain a suspension; drying the suspension to obtain a white powder; adding a mixed solution of hydrogen peroxide and sodium hydroxide to the white powder, and ultrasonically treating the white powder to obtain a titanium peroxide solution;
[0028] And / or, the volume ratio of water to alcohol is (0.1-10):1, preferably (0.1-1):1;
[0029] And / or, a hydrogen peroxide solution and a sodium hydroxide solution are mixed in a volume ratio of (0.1-10):1 to obtain a hydrogen peroxide and sodium hydroxide mixed solution, wherein the concentration of the hydrogen peroxide solution is 30-100 wt %, and the concentration of the sodium hydroxide solution is 0.1-10 mol / L. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The catalyst Bi prepared in Example 1 0.5 Y 0.5 XRD pattern of VO4 solid solution;
[0031] Figure 2 is a flow chart of the preparation of the titanium peroxide solution in Example 1;
[0032] Figure 3 (a) XRD spectrum and (b) UV-Vis spectrum of the amorphous titanium oxide powder in Example 1;
[0033] Figure 4 The loaded Pt and amorphous TiO prepared in Example 1 x Bi of the coating 0.5 Y 0.5 TEM image of VO4;
[0034] Figure 5 is the UV-Vis spectrum of the catalyst;
[0035] Figure 6 This is a performance comparison chart of catalysts for photocatalytic decomposition of pure water to produce hydrogen. DETAILED DESCRIPTION
[0036] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to be used to explain the present invention, but should not be understood as limiting the present invention.
[0037] TiO in the embodiment of the present invention xA photocatalyst coated with vanadate, the photocatalyst comprising vanadate and TiO x The coating layer, the surface of the vanadate is loaded with precious metals, the TiO x The coating layer covers the surfaces of the vanadate and the noble metal.
[0038] TiO in the embodiment of the present invention x The vanadate-coated photocatalyst loads precious metals on the surface of the vanadate, which can effectively reduce the recombination probability of electrons and holes and improve the activity of the catalyst; a uniform amorphous titanium oxide coating layer is formed on the surface of the photocatalyst, which can effectively inhibit the occurrence of hydrogen-oxygen recombination reactions on the surface of the co-catalyst and improve the efficiency of photocatalytic water decomposition to produce hydrogen.
[0039] In some embodiments, preferably, the vanadate is bismuth yttrium vanadate, whose chemical formula is Bi x Y 1-x VO4, of which 0.1 <x<0.9。
[0040] In some embodiments, preferably, the noble metal includes at least one of gold, palladium, platinum or rhodium. Preferably, the loading amount of the noble metal is 0.1 to 1 wt %, based on the total mass of the photocatalyst.
[0041] In the embodiments of the present invention, the type and amount of the precious metal are further optimized. Within this amount range, the precious metal co-catalyst can be evenly loaded on the surface of the catalyst, effectively improving the activity of the catalyst. If the amount of the precious metal is too low, the improvement in the activity of the catalyst is very limited. If the amount of the precious metal is too high, it may aggregate on the surface of the catalyst, which is not conducive to further improving the activity of the catalyst.
[0042] In some embodiments, preferably, the TiO x The thickness of the layer is 1 to 6 nm. Preferably, the loading amount of Ti is 1 to 10 wt.%, based on the total mass of the photocatalyst.
[0043] In the embodiment of the present invention, the dosage of the titanium peroxide solution is preferably selected, that is, the amorphous TiO x A uniform coating layer with appropriate thickness is formed on the surface of the co-catalyst, which can effectively inhibit the occurrence of hydrogen-oxygen recombination reaction on the surface of the co-catalyst while ensuring the efficiency of photocatalytic decomposition of water to produce hydrogen; if the amount of titanium peroxide solution is too small, it is not enough to form a complete and uniform TiO2 coating on the surface of the co-catalyst. x The coating layer has a very limited inhibitory effect on the hydrogen-oxygen complex reaction. If the amount of titanium peroxide solution is too much, the TiO x If the coating layer is too thick, the activity of the catalyst may be reduced.
[0044] The embodiment of the present invention also provides a TiO x The preparation method of the photocatalyst coated with vanadate comprises the following steps:
[0045] (1) dispersing vanadate in water, adding a noble metal salt solution, and irradiating with ultraviolet light under a vacuum environment to obtain a first suspension;
[0046] (2) adding a titanium peroxide solution to the first suspension obtained in step (1), and irradiating the suspension with ultraviolet light under a vacuum environment to obtain a second suspension;
[0047] (3) filtering, washing and drying the second suspension obtained in step (2) to obtain TiO x Encapsulated vanadate photocatalysts.
[0048] TiO in the embodiment of the present invention x The method for preparing a photocatalyst coated with vanadate comprises loading a noble metal co-catalyst on the surface of the catalyst by ultraviolet irradiation under a vacuum environment, selectively anchoring the noble metal atoms on the catalytic site or electron aggregation area on the surface of the photocatalyst, and reducing the migration distance of photogenerated electrons; uniformly coating amorphous TiO on the surface of the vanadate by photoreduction of soluble titanium peroxide x , the formed TiO x It can effectively inhibit the occurrence of hydrogen-oxygen recombination reaction on the catalyst surface and improve the efficiency of photocatalytic water decomposition to produce hydrogen; the process is simple, the raw materials are cheap, and it does not involve complex processes such as chemical vapor deposition, physical vapor deposition and atomic deposition, which is convenient for promotion and application in industrial production.
[0049] In some embodiments, preferably, in step (1), the precious metal salt includes at least one of chloroauric acid, palladium trichloride, chloroplatinic acid and rhodium trichloride; and / or, in step (1) and / or (2), the pressure of the vacuum environment is 0.1 to 1 KPa.
[0050] In the embodiment of the present invention, it is preferred that the ultraviolet irradiation is carried out in a vacuum environment, so that the precious metal co-catalyst and the vanadate and the TiO x The coating layer has a stronger binding force with the photocatalyst, which can increase the service life of the photocatalyst.
[0051] In some embodiments, preferably, in step (1) and / or (2), the wavelength of the ultraviolet light source is 200-400 nm, and the light intensity is 10-100 mW / cm 2 , the irradiation time is 1 to 3 hours.
[0052] In the embodiments of the present invention, the wavelength, intensity and irradiation time of ultraviolet rays are optimized, and the deposition rate and morphology of the co-catalyst or coating can be controlled. If the light intensity is too high, it is not conducive to the uniform deposition of the precious metal co-catalyst and titanium oxide on the surface of the vanadate, and it is easy to cause surface particle agglomeration. If the light intensity is too low, it is not conducive to the deposition of the precious metal co-catalyst and titanium oxide on the surface of the vanadate.
[0053] In some embodiments, preferably, in step (1), the vanadate photocatalyst is tetragonal zircon phase bismuth yttrium vanadate, and the preparation method thereof comprises the following steps:
[0054] A. dissolving bismuth salt, yttrium salt and vanadium salt in nitric acid solution, adding ammonia water to adjust the pH, and reacting to obtain a precipitate;
[0055] B. subjecting the precipitate obtained in step A to static aging, solid-liquid separation, washing and drying to obtain a solid powder;
[0056] C. calcining the solid powder obtained in step B to obtain tetragonal zircon phase bismuth yttrium vanadate.
[0057] In an embodiment of the present invention, a low-crystalline tetragonal bismuth yttrium vanadate solid solution with uniformly distributed elements is first synthesized by a liquid phase co-precipitation method, and then the crystallinity is improved by high-temperature calcination, which can avoid the problem of photogenerated carrier recombination and improve the efficiency of photocatalytic water decomposition to produce hydrogen.
[0058] In some embodiments, preferably, in step A, the molar ratio of the bismuth salt to the yttrium salt is (0.1-10):1, and the molar ratio of the total amount of the bismuth salt and the yttrium salt to the vanadium salt is (0.1-10):1; and / or, the pH is adjusted to 4-12;
[0059] And / or, in step C, the calcination temperature is 400-1000°C, and the calcination time is 2-12h. Further preferably, in step A, the ratio of the bismuth salt to the yttrium salt is 0.3-1, and the ratio of the total amount of the bismuth salt and the yttrium salt to the vanadium salt is 0.5-1; and / or, the pH is adjusted to 7-8; and / or, in step C, the calcination temperature is 500-600°C. More preferably, the concentration of the ammonia water is 25-30%.
[0060] In the embodiment of the present invention, the dosage ratio of bismuth salt, yttrium salt and vanadium salt is optimized, and an appropriate amount of yttrium atoms is used to maintain the metastable tetragonal bismuth vanadate structure and inhibit the formation of thermodynamically stable monoclinic bismuth vanadate, thereby generating a pure phase vanadate solid solution; the pH range is further optimized to prevent the direct formation of hydroxide precipitation in high pH solutions and the formation of irregular amorphous products at low pH values.
[0061] In some embodiments, preferably, in step A, the bismuth salt and / or yttrium salt includes at least one of chloride, nitrate, sulfate, organic acid salt or alkoxide; the vanadium salt includes at least one of ammonium metavanadate, sodium orthovanadate or vanadium chloride; and / or the concentration of the nitric acid solution is 0.1 to 10 mol / L, and / or, after the bismuth salt, yttrium salt and vanadium salt are dissolved in the nitric acid solution, the total concentration of metal salts in the solution is 0.1 to 1 mol / L.
[0062] In some embodiments, preferably, in step B, the solid-liquid separation is performed by centrifugal separation. Further preferably, the rotation speed of the centrifugal separation is 3000-10000 rpm, and the time of the centrifugal separation is 1-10 min.
[0063] In some embodiments, preferably, in the step B, the solvent used for the cleaning includes at least one of water, ethanol and acetone.
[0064] In some embodiments, preferably, in step (2), the preparation process of the titanium peroxide solution comprises: adding a titanium salt to a mixed solution of water and alcohol to react to obtain a suspension; drying the suspension to obtain a white powder; adding a mixed solution of hydrogen peroxide and sodium hydroxide to the white powder, and ultrasonically treating the white powder to obtain a titanium peroxide solution;
[0065] And / or, the volume ratio of water to alcohol is (0.1-10):1, preferably (0.1-1):1;
[0066] And / or, a hydrogen peroxide solution and a sodium hydroxide solution are mixed in a volume ratio of (0.1-10):1 to obtain a hydrogen peroxide and sodium hydroxide mixed solution, wherein the concentration of the hydrogen peroxide solution is 30-100 wt %, and the concentration of the sodium hydroxide solution is 0.1-10 mol / L.
[0067] In some embodiments, preferably, the titanium salt includes at least one of titanium tetrachloride, isopropyl titanate, tetrabutyl titanate, titanium isooctylate, and tetraethyl titanate; and / or the alcohol includes at least one of methanol, ethanol, isopropanol, and n-butanol.
[0068] The technical solution of the present invention is described in detail below in conjunction with specific embodiments and drawings.
[0069] Example 1
[0070] Bi 0.5 Y 0.5 The synthesis steps of VO4 nano-photocatalyst are as follows:
[0071] (1) Weigh 2.5 mmol of bismuth nitrate pentahydrate and 2.5 mmol of yttrium nitrate hexahydrate and dissolve them in 50 mL of 2 mol / L dilute nitric acid solution;
[0072] (2) quickly adding 4 mL of 28% ammonia water, then slowly adding 28% ammonia water until the pH reaches 7. After stirring for 2 h, the precipitate is allowed to stand and age for 2 h.
[0073] (3) After the white precipitate is washed by centrifugation, it is dried in a constant temperature forced air drying oven at 80° C. for 12 h to obtain a white powder;
[0074] (4) After grinding the white powder, calcining it in a muffle furnace at 550°C for 6 h at a heating rate of 5°C / min;
[0075] (5) After cooling naturally to room temperature, the light yellow powder obtained is tetragonal zircon phase Bi 0.5 Y 0.5 VO4 solid solution.
[0076] Bi 0.5 Y 0.5 XRD patterns of VO4 photocatalysts Figure 1 As shown in the figure, it can be seen that the crystal structure of the catalyst exhibits a pure tetragonal zircon phase and no impurities are detected.
[0077] The preparation process of titanium peroxide solution is as follows: Figure 2 As shown, the steps are as follows:
[0078] (1) 9 mL of isopropyl titanate was added dropwise into a mixed solution consisting of 85 mL of isopropyl alcohol and 15 mL of water, and the solution temperature was controlled at 40° C. to obtain a suspension;
[0079] (2) The suspension was dried in an oven at 60°C until the solvent was completely evaporated. The resulting white powder was amorphous TiO x H y ;
[0080] (3) Weigh 12 mg of amorphous TiO x H y Then, a mixed solution of 2 mL 30% H2O2 and 0.3 mL 1 mmol / L NaOH was added, and the yellow solution obtained after ultrasonic treatment for 5 seconds was the titanium peroxide solution.
[0081] Amorphous TiO x H y The XRD pattern of Figure 3 As shown in a, the UV-Vis spectrum is Figure 3 As shown in b, it can be seen from the figure that TiO x H yThere is no obvious crystalline phase; the obtained powder has a single absorption edge, no obvious impurity energy level, and has a high purity.
[0082] TiO x The steps of coating the photocatalyst are as follows:
[0083] (1) 0.1gBi 0.5 Y 0.5 VO4 powder was dispersed in 100 mL of ultrapure water by ultrasonication, and then chloroplatinic acid aqueous solution was added to react Pt with Bi. 0.5 Y 0.5 The mass ratio of VO4 is 1:200;
[0084] (2) Then, the solution in step 1 was added to a 280 mL Pyrex glass reactor, and the vacuum degree in the reactor was reduced to 0.6 kPa using a mechanical pump. The solution was irradiated under a xenon lamp for 2 h. The xenon lamp had an irradiation wavelength of 300 to 400 nm, and the incident light intensity was controlled at 100 mW / cm 2 Then, the vacuum in the reactor was vented to normal pressure to obtain Bi 0.5 Y 0.5 VO4-Pt dispersion;
[0085] (3) Add 2 mL of titanium peroxide solution to Bi 0.5 Y 0.5 In the VO4-Pt dispersion, the vacuum degree in the reactor was reduced to 0.6 kPa using a mechanical pump, and the solution was irradiated under a xenon lamp for 2 h. The illumination wavelength was 300-400 nm, and the intensity of the incident light was controlled at ~100 mW / cm 2 Then, the vacuum in the reactor was vented to normal pressure to obtain Bi 0.5 Y 0.5 VO4-Pt@TiO δ Dispersion liquid;
[0086] (4) After the dispersion in step 3 is filtered, washed and dried, the light grey powder obtained is Bi 0.5 Y 0.5 VO4-Pt@TiO δ .
[0087] The Bi prepared in this embodiment 0.5 Y 0.5 VO4-Pt@TiO δ TEM Figure 4 As shown in the figure, it can be seen that the catalyst Pt is evenly dispersed in Bi 0.5 Y 0.5 VO4 surface, and the thickness is about 4nm amorphous TiO x The coating is evenly coated on the catalyst.
[0088] Since UV-Vis is sensitive to the composition and properties of the material surface, TiO x The coating coverage can be further verified by UV-Vis characterization. Figure 5 As shown, Bi 0.5 Y 0.5 VO4 has no light absorption performance in the region above 400nm; after loading metal Pt, the absorption in the visible light region is significantly enhanced; due to TiO x No visible light absorption properties (such as Figure 3 b), so in Bi 0.5 Y 0.5 The VO4-Pt surface is further coated with TiO x After that, the visible absorption performance of the photocatalyst dropped significantly, further proving that TiO x Full coverage of the surface Pt particles is achieved, thereby achieving the effect of passivating the hydrogen-oxygen recombination sites on the catalyst.
[0089] Example 2
[0090] The method is the same as that of Example 1, except that: TiO x In the step (2) and step (3) of coating the photocatalyst, the illumination wavelength is 350-400 nm, and a TiO layer with a thickness of about 1 nm is formed. x The sample is denoted as Bi 0.5 Y 0.5 VO4-Pt@TiOx-1.
[0091] Example 3
[0092] The method is the same as that of Example 1, except that: TiO x In the step (3) of coating the photocatalyst, the amount of titanium peroxide solution added is 1 mL, and a TiO x The sample is denoted as Bi 0.5 Y 0.5 VO4-Pt@TiOx-2.
[0093] Comparative Example 1
[0094] The preparation method of this comparative example is the same as that of Example 1, except that: x In the step (3) of coating the photocatalyst, a TiOx coating is coated on the surface of the photocatalyst by an immersion method, and 2 mL of titanium peroxide solution is added to the Bi 0.5 Y 0.5After the VO4-Pt dispersion was added, the solution was placed in an 80°C water bath, stirred and evaporated to dryness, and then the powder was collected and placed in an 80°C oven to dry overnight, and finally calcined in a muffle furnace at 450°C in air atmosphere for 2 hours. The collected powder was Bi 0.5 Y 0.5 VO4-Pt@TiOx(WI).
[0095] Comparative Example 2
[0096] In this comparative example, only Bi 0.5 Y 0.5 VO4-Pt, without TiO x The coating preparation method is the same as that in Example 1.
[0097] Comparative Example 3
[0098] In this comparative example, only Bi 0.5 Y 0.5 VO4, without Pt loading, is prepared in the same manner as in Example 1.
[0099] Comparative Example 4
[0100] In this comparative example, Bi 0.5 Y 0.5 VO4-Pt@Cr2O3, it is only necessary to replace the titanium peroxide solution in step 3 with 0.5mL 0.1M K2CrO4 solution, and the rest of the preparation method is the same as that in Example 1.
[0101] Comparative Example 5
[0102] The method is the same as that of Example 1, except that: in step (2) and step (3) of coating the photocatalyst with the TiOx coating, the process is carried out under non-vacuum conditions, and no amorphous titanium oxide coating layer is observed on the surface.
[0103] Experimental example
[0104] The catalysts prepared in the examples and comparative examples were used for photocatalytic complete decomposition of water to produce hydrogen. The test steps are as follows and the test results are shown in Figure 6 and Table 1.
[0105] (1) Weigh 0.1 g of the catalyst and disperse it in 100 mL of ultrapure water by ultrasonication, then add the dispersion into a Pyrex glass reactor:
[0106] (2) Use a mechanical pump to reduce the vacuum in the reactor to 0.6 kPa, then irradiate the solution under a xenon lamp with a wavelength of 300 to 850 nm and an incident light intensity of ~100 mW / cm 2 ;
[0107] (3) The hydrogen and oxygen contents in the reactor were tested by gas chromatography every hour.
[0108] like Figure 6 As shown, the Bi of Comparative Example 3 without Pt catalyst 0.5 Y 0.5 VO4 has no photocatalytic OWS activity; after loading Pt in Comparative Example 2, the OWS hydrogen production activity is 31.9 μmol / h; while in Example 1, after further coating amorphous TiO x After coating, the hydrogen production activity of OWS was significantly improved to 60.4 μmol / h.
[0109] Table 1
[0110]
[0111]
[0112] From the data in Table 1, it can be seen that the catalyst Bi prepared in Example 1 0.5 Y 0.5 The hydrogen production activity of VO4-Pt@TiOx is 60.4 μmol / h, and the oxygen production activity is 30.2 μmol / h. The thickness of the catalyst TiOx coating prepared in Example 2 and Example 3 is reduced, resulting in a corresponding decrease in the hydrogen production activity and the oxygen production activity, but it can still meet the use requirements.
[0113] The catalyst Bi prepared by the impregnation method in Comparative Example 1 0.5 Y 0.5 VO4-Pt@TiOx(WI) makes the TiOx coating layer uneven and not tightly bound to the vanadate surface, resulting in a hydrogen production activity of only 14.0μmol / h and an oxygen production activity of only 7.0μmol / h, which cannot meet the needs of use.
[0114] After 100 hours of continuous illumination, the performance of the coated photocatalyst in Example 1 was tested again, and the hydrogen production activity was 58.9 μmol / h, which was still within the normal test performance fluctuation range of this experiment (60.4±3.6 μmol / h). 0.5 Y 0.5 The initial hydrogen production activity of VO4-Pt@Cr2O3 is 62.2 μmol / h, which decays to 46.7 μmol / h after 100 hours of illumination. Therefore, the amorphous TiOx coating prepared by the present invention exhibits good light corrosion resistance.
[0115] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0116] Although the above embodiments have been shown and described, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. Changes, modifications, substitutions and variations of the above embodiments by those of ordinary skill in the art are all within the scope of protection of the present invention.
Claims
1. A TiO x A method for preparing a photocatalyst coated with vanadate, It is characterized in that The following steps are involved: (1) dispersing vanadate in water, adding a noble metal salt solution, and irradiating with ultraviolet light under a vacuum environment to obtain a first suspension; (2) adding a titanium peroxide solution to the first suspension obtained in step (1), and irradiating the suspension with ultraviolet light under a vacuum environment to obtain a second suspension; (3) filtering, washing and drying the second suspension obtained in step (2) to obtain TiO x coated vanadate photocatalysts; The prepared photocatalyst includes vanadate and TiO x The coating layer, the surface of the vanadate is loaded with precious metals, the TiO x The coating layer covers the surfaces of the vanadate and the noble metal.
2. TiO according to claim 1 x A method for preparing a photocatalyst coated with vanadate, It is characterized in that The vanadate is bismuth yttrium vanadate, and its chemical formula is Bi x Y 1-x VO 4 , where 0.1 <x<0.9。 3. TiO according to claim 1 x A method for preparing a photocatalyst coated with vanadate, It is characterized in that The noble metal includes at least one of gold, palladium, platinum or rhodium.
4. TiO according to claim 1 or 3 x A method for preparing a photocatalyst coated with vanadate, It is characterized in that The loading amount of the noble metal is 0.1 to 1 wt %, based on the total mass of the photocatalyst.
5. TiO according to claim 1 x A method for preparing a photocatalyst coated with vanadate, It is characterized in that The TiO x The thickness of the coating layer is 1 to 6 nm.
6. TiO according to claim 1 or 5 x A method for preparing a photocatalyst coated with vanadate, It is characterized in that The loading amount of Ti is 1 to 10 wt.%, based on the total mass of the photocatalyst.
7. The TiO according to claim 1 x A method for preparing a photocatalyst coated with vanadate, It is characterized in that In the step (1), the noble metal salt comprises at least one of chloroauric acid, palladium trichloride, chloroplatinic acid and rhodium trichloride; And / or, in the steps (1) and / or (2), the pressure of the vacuum environment is 0.1-1 KPa.
8. The TiO according to claim 1 x A method for preparing a photocatalyst coated with vanadate, It is characterized in that In the steps (1) and / or (2), the wavelength of the ultraviolet light source is 200 to 400 nm, and the light intensity is 10 to 100 mW / cm 2 , the irradiation time is 1 to 3 hours.
9. The TiO according to claim 1 x A method for preparing a photocatalyst coated with vanadate, It is characterized in that In the step (1), the vanadate photocatalyst is tetragonal zircon phase bismuth yttrium vanadate, and the preparation method thereof comprises the following steps: A. dissolving bismuth salt, yttrium salt and vanadium salt in nitric acid solution, adding ammonia water to adjust the pH, and reacting to obtain a precipitate; B. subjecting the precipitate obtained in step A to static aging, solid-liquid separation, washing and drying to obtain a solid powder; C. calcining the solid powder obtained in step B to obtain tetragonal zircon phase bismuth yttrium vanadate.
10. The TiO according to claim 9 x A method for preparing a photocatalyst coated with vanadate, It is characterized in that In the step A, the molar ratio of the bismuth salt to the yttrium salt is (0.1-10):1, and the molar ratio of the total amount of the bismuth salt and the yttrium salt to the vanadium salt is (0.1-10):1; and / or, the pH is adjusted to 4-12; And / or, in the step C, the calcination temperature is 400-1000° C., and the calcination time is 2-12 hours.
11. The TiO according to claim 1 x A method for preparing a photocatalyst coated with vanadate, It is characterized in that In the step (2), the preparation process of the titanium peroxide solution comprises: adding titanium salt to a mixed solution of water and alcohol to react to obtain a suspension; drying the suspension to obtain a white powder; adding a mixed solution of hydrogen peroxide and sodium hydroxide to the white powder, and ultrasonically treating the white powder to obtain a titanium peroxide solution; And / or, the volume ratio of water to alcohol is (0.1-10):1; And / or, a hydrogen peroxide solution and a sodium hydroxide solution are mixed in a volume ratio of (0.1-10):1 to obtain a hydrogen peroxide and sodium hydroxide mixed solution, wherein the concentration of the hydrogen peroxide solution is 30-100 wt %, and the concentration of the sodium hydroxide solution is 0.1-10 mol / L.
12. The TiO according to claim 11 x A method for preparing a photocatalyst coated with vanadate, It is characterized in that The volume ratio of water to alcohol is (0.1-1):1.