Semi-dry desulfurization ash-fly ash-slag composite cementitious material and preparation method thereof

Through the preparation of semi-dry desulfurization ash-fly ash-slag composite cementitious materials, the problems of low heavy metal removal rate and high energy consumption in the existing technology are solved, and the effects of efficient solidification and compressive strength in line with national standards are achieved. Solved the problem of water environment pollution.

CN116986829BActive Publication Date: 2024-10-29CHINA UNIV OF GEOSCIENCES (WUHAN) +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310698914.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-13
Publication Date
2024-10-29
Estimated Expiration
2043-06-13

AI Technical Summary

Technical Problem

The existing technology has a low heavy metal removal rate and consumes a large amount of energy materials when treating wastewater containing cadmium and lead, making it difficult to effectively solve the problem of water environment pollution.

Method used

Semi-dry desulfurization ash-fly ash-slag composite cementitious material is used to form a cementitious material that meets concrete standards by combining fly ash, slag and semi-dry desulfurization ash with an alkali activator, using activators and wastewater Uniform mixing and curing are performed to generate composite materials with high compressive strength and achieve solidification of heavy metals.

Benefits of technology

It achieves effective solidification of heavy metals Pb2+ and Cd2+, reduces the leaching toxicity of heavy metals, meets the compressive strength of concrete national standards, does not require additional energy substances, and significantly improves the efficiency and effect of wastewater treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116986829B_ABST
    Figure CN116986829B_ABST
Patent Text Reader

Abstract

The present invention discloses a semi-dry desulfurization ash-fly ash-slag composite cementitious material and a preparation method thereof. The present invention comprises the following raw materials: fly ash + slag: 50%, semi-dry desulfurization ash: 3% to 9%, alkali activator 5% to 20%, and waste water 20.1% to 29.5%, wherein the mass ratio of fly ash to slag is 0.4 to 2.3:1. The preparation method comprises sieving the semi-dry desulfurization ash, slag, and fly ash of the above-mentioned mass percentages and mixing them evenly, then adding a certain amount of waste water, and then adding the prepared activator solution and stirring evenly, pouring into a mold, shaking, standing, demolding and curing. The semi-dry desulfurization ash-fly ash-slag composite cementitious material of the present invention can effectively solidify the heavy metal Pb in the wastewater at the same time. 2+ 、Cd 2+ It does not require additional energy consumption, meets national concrete standards, has low heavy metal leaching toxicity, and is highly environmentally safe.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inorganic gelling materials, and in particular to a semi-dry desulfurization ash-fly ash-slag composite gelling material and a preparation method thereof. Background Art

[0002] Industrial wastewater refers to wastewater discharged during the production process of industrial enterprises. The wastewater contains wastes from the production process, pollutants such as lost raw materials, intermediate products, final products, and by-products, and is the main source of water pollution. With the continuous development of chemical, smelting, electroplating and other industrial production, the amount of cadmium, lead and their compounds is increasing day by day, and the polluted wastewater containing cadmium and lead discharged is becoming more and more serious, and has now become one of the most harmful industrial wastewaters in the world. Traditional methods for treating lead and cadmium wastewater mainly include chemical precipitation, ion exchange, electrolysis, reverse osmosis, electrodialysis, activated carbon adsorption, biological adsorption, etc., among which the heavy metal removal rate of most methods is only about 90%. Moreover, most of these methods in the prior art consume energy substances to remove heavy metals from wastewater. Summary of the invention

[0003] The object of the present invention is to provide a semi-dry desulfurization ash-fly ash-slag composite cementitious material and a preparation method thereof in view of the above-mentioned deficiencies in the prior art.

[0004] The semi-dry desulfurization ash-fly ash-slag composite cementitious material of the present invention comprises the following raw materials in percentage by mass: fly ash+slag: 50%, semi-dry desulfurization ash: 3%-9%, alkali activator 5%-20%, waste water 20.1%-29.5%; wherein the mass ratio of fly ash to slag is 0.4-2.3:1.

[0005] Furthermore, the alkaline activator is NaOH and sodium water glass Na2O·nSiO2.

[0006] Furthermore, the modulus of the alkaline activator is 0.5 to 2.0.

[0007] As mentioned above, in the preparation method of the semi-dry desulfurization ash-fly ash-slag composite cementitious material, the semi-dry desulfurization ash, slag and fly ash in the above-mentioned mass percentages are sieved and mixed evenly, and then a certain amount of waste water is added, and then the prepared activator is added and stirred evenly, poured into a mold, shaken, allowed to stand, demolded and cured to obtain the semi-dry desulfurization ash-fly ash-slag composite cementitious material.

[0008] Furthermore, the semi-dry desulfurization ash, slag and fly ash are sieved through a 120-mesh sieve.

[0009] Furthermore, the alkaline activator is NaOH and sodium water glass Na2O·nSiO2; the preparation process of the alkaline activator solution is as follows: weigh sodium hydroxide in a beaker, add an appropriate amount of distilled water and stir to dissolve, add water glass after cooling, stir and let stand to obtain the alkaline activator solution.

[0010] Further, cover with plastic wrap and let stand for 24 hours.

[0011] The semi-dry desulfurization ash-fly ash-slag composite cementitious material of the present invention uses solid waste as the main raw material, and does not require additional energy-consuming substances to treat wastewater, so as to obtain a cementitious material that meets the national standard for concrete; when fly ash (FA) and slag (Sg) are added at the same time, the activity of the slag is first stimulated, and the released heat can stimulate the fly ash more quickly, thereby improving the volcanic ash effect of the fly ash. In addition, the semi-dry desulfurization ash (FGD) contains a large amount of SO3, which has a stimulating effect on the volcanic ash effect of the fly ash. The fly ash undergoes a hydration reaction under the sulfate activity stimulation effect of the desulfurization ash, and the generated needle-shaped crystal calcium aluminate is crossed and filled with other hydration products, which can increase the compressive strength of the cementitious material. At different ages, not only does the strength meet the national standard for concrete, but the heavy metal leaching toxicity is also low, achieving the heavy metal Pb 2+ 、Cd 2+ effective curing. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Picture 1 The present invention is a flow chart of the preparation and testing of the semi-dry desulfurization ash-fly ash-slag composite cementitious material. DETAILED DESCRIPTION

[0013] The following are specific embodiments of the present invention, which further describe the technical solutions of the present invention, but the present invention is not limited to these embodiments.

[0014] 1. Implementation plan:

[0015] 3.1.1 Technical solution (taking the cementitious material of the present invention as an example)

[0016] (1) Preparation of cementitious materials:

[0017] Add 3% Pb 2+ 、Cd 2+ (added in the form of nitrate) to simulate heavy metal-containing wastewater, an orthogonal experiment was used to select five factors: water-binder ratio, activator modulus, activator content, fly ash to slag ratio, and desulfurization ash content. Each factor was set at four levels, and 16 groups of orthogonal experiments were conducted. The factor levels are shown in Table 1. Picture 1 The process was to prepare several 20cm×20cm×20cm samples and cure them for 7 and 28 days respectively. 2+ 、Cd2+ Leaching concentration, select the best experimental ratio.

[0018] Table 1 Orthogonal experimental factor level table

[0019]

[0020] (2) Heavy metal solidification experiment

[0021] According to Tables 2 and 3, simulated wastewater with different contents of heavy metals Cd(Ⅱ) and Pb(Ⅱ) were prepared, and cementitious materials were prepared according to the optimal formula.

[0022] Table 2 Cd content setting in simulated wastewater

[0023] CD-0 CD-1 CD-2 Cd-3 CD-4 CD-5 0% 0.5% 1% 2% 3% 4%

[0024] Table 3 Pb content setting in simulated wastewater

[0025] Pb-0 Pb-1 Pb-2 Pb-3 Pb-4 Pb-5 0% 0.5% 1% 2% 3% 4%

[0026] in:

[0027] The Cd curing experiment started at 11:15 am on November 23, 2021, and the Pb curing experiment started at 10.25 am on November 25, 2021. Each group was freeze-dried and cured for 7 and 28 days, and performance tests were carried out at different times.

[0028] (3) Performance test:

[0029] A. Curing performance-heavy metal leaching test

[0030] The block samples after freeze-drying for 7 days and 28 days were crushed, and then the samples were passed through 7-mesh and 16-mesh sieves (1.19mm-2.80mm). 10g of sample particles after screening were placed in a 250mL conical flask and 100mL of secondary water (solid-liquid ratio 1:10) was added. The mouth of the conical flask was sealed with plastic wrap. The conical flask was fixed in a digital water bath constant temperature oscillator and oscillated for 8 hours at a frequency of 120r / min. After the oscillation, it was allowed to stand for 16 hours. The leachate was filtered with a microporous filter membrane (0.45μm). The obtained leachate was diluted twice with 2% HNO3 and the concentration of heavy metal ions in the leachate was tested by ICP. The neutral environment leaching test was carried out in accordance with HJ557-2010.

[0031] B. Mechanical properties-compressive strength test

[0032] The prepared cementitious material slurry was placed in a 20mm×20mm×20mm triple metal test mold to make a test block. After standing for 1 day, the film was removed and numbered, and then the test block samples were sealed and placed in a standard curing room with a relative humidity of more than 90% and a temperature of (20±2)℃ for continued curing for 3, 7, 14, and 28 days. The unconfined compressive strength tests were performed respectively in accordance with the steps in the "Test Procedure for Stabilized Materials of Inorganic Binders for Highway Engineering" (JTGE51-2009).

[0033] 3.1.2. Cementitious material formula

[0034] Cementitious material A (cementitious material of the present invention):

[0035] Water-binder ratio: 0.46; alkali activator modulus: 0.5; water glass: 20.95g; NaOH: 9.82g; FA: 31.80g; Sg: 74.8g; FGD: 10g; simulated wastewater: 50.98g;

[0036] Cementitious material B:

[0037] Alkali activator modulus: 0.5; water glass: 20.95g; NaOH: 9.82g; Sg: 91.6g; FGD: 13.2g; simulated wastewater: 65.34g;

[0038] Cementitious material C:

[0039] Alkali activator modulus: 0.5; water glass: 20.95g; NaOH: 9.82g; FA: 56.8g; FGD: 18.97g; simulated wastewater: 95.8g;

[0040] Cementitious material D:

[0041] Alkali activator modulus: 0.5; water glass: 20.95g; NaOH: 9.82g; FA: 34.4g; Sg: 79.3g; simulated wastewater: 56.5g;

[0042] Cementitious material E:

[0043] Rice husk ash: 18.4g; CFB desulfurization ash: 113g; Steel slag powder: 55.5g; Activator: 25.4g; Simulated wastewater: 100g;

[0044] Cementitious material F:

[0045] Slag: 167g; desulfurized ash: 28.6g; limestone: 4.4g; active activator: 4.85g; simulated wastewater: 100g.

[0046] Cementitious material A is a ternary composite material of the present invention; cementitious materials B, C and D are binary composite materials obtained by reducing one raw material from A; cementitious materials E and F are other common composite materials.

[0047] The invention provides a ternary composite cementitious material for solidifying heavy metals Pb(II) and Cd(II) in industrial wastewater. After corresponding curing age, the heavy metal leaching rate is lower than that in existing research, and the compressive strength meets national standards.

[0048] 3.1.3. Preparation process of cementitious materials

[0049] Weigh sodium hydroxide in a beaker, add appropriate amount of distilled water, stir to dissolve, cool → add water glass, stir and let stand → semi-dry desulfurization ash, slag, fly ash, etc. through a 120-mesh sieve, stir evenly → add a certain amount of waste water → weigh the activator (NaOH+Na2O.nSiO2) and pour it into the mixture, stir for 5 minutes → pour into the mold, shake, cover with plastic wrap → wait 24 hours, demold → put in a standard curing box for curing.

[0050] 3.2 Effect after implementation

[0051] 3.2.1. Implementation and Comparison

[0052] Table 4 Pb leaching test (unit: μg / l)

[0053]

[0054]

[0055] Table 5 Cd leaching test (unit: μg / l)

[0056]

[0057] As shown in Tables 4 and 5, the Pb of Group 9 2+ 、Cd 2+ The 7d and 28d leaching toxicities of heavy metals are both the lowest, and the leaching amounts are far lower than the limits specified in the national standard GB5085.3-2001 "Hazardous Waste Identification Standard-Leaching Toxicity Identification" (Pb<5mg / L, Cd<1mg / L). Taking into account the economic cost and the plasticity of the cementitious material, the ninth group of formulas was selected as the preparation conditions of the cementitious material of the present invention, and subsequent heavy metal solidification performance comparison, compressive strength test and other experiments were carried out.

[0058] 3.2.2 Performance Testing

[0059] A. Curing performance-heavy metal leaching test

[0060] Table 6 Leaching test of simulated wastewater containing Cd for 7 days (unit: μg / l)

[0061]

[0062] Table 7 Leaching test of simulated wastewater containing Pb for 7 days (unit: μg / l)

[0063]

[0064]

[0065] Table 8 Leaching test of simulated wastewater containing Cd for 28 days (unit: μg / l)

[0066]

[0067] Table 9 Leaching test of simulated wastewater containing Pb for 28 days (unit: μg / l)

[0068]

[0069] As shown in Tables 6 to 9, as the heavy metal content in the simulated wastewater increases, its leaching concentration also increases. Under neutral conditions (PH = 7), in the gelling material of the present invention: 4% Pb 2+ , 7 days and 28 days Pb 2+ The curing rates are 99.75% and 99.95% respectively; adding 4% Cd 2+ , 7-day and 28-day Cd 2+ The solidification rates of the leaching materials are 99.99% and 99.99% respectively, and the leaching amounts are far lower than the limit values ​​specified in the national standard GB5085.3-2001 "Hazardous Waste Identification Standard - Leaching Toxicity Identification" (Pb<5mg / L, Cd<1mg / L). It can be seen that the 4% lead and cadmium cementing materials do not have leaching toxicity. At the same time, the leaching amount of heavy metals is high at 7 days, but with the increase of curing time, the leaching amount at 28 days is reduced, indicating that Pb 2+ and Cd 2+ During the curing process, it is solidified inside the cementitious material. By comparing groups A, B, C, and D, it can be seen that the ternary system (fly ash, slag, and semi-dry desulfurization ash) proposed in the present invention has a good effect of solidifying heavy metals in wastewater, and its solidification effect is better than that of the binary system; by comparing groups A, E, and F, it can be seen that the cementitious material of the present invention solidifies heavy metals Cd 2+ , Pb 2+ The effect is better than other common types of cementitious materials.

[0070] B. Mechanical properties-compressive strength test

[0071] Table 10 Comparison of compressive properties

[0072]

[0073] Table 11 3d compressive strength test of simulated wastewater containing Pb heavy metals (unit: Mpa)

[0074]

[0075] Table 12 3d compressive strength test of simulated wastewater containing Cd heavy metals (unit: Mpa)

[0076]

[0077] Table 13 Compressive strength test of simulated wastewater containing Pb for 7 days (unit: Mpa)

[0078]

[0079] Table 14 Compressive strength test of simulated wastewater containing Cd for 7 days (unit: Mpa)

[0080]

[0081] Table 15 Compressive strength test of simulated wastewater containing Pb for 14 days (unit: Mpa)

[0082]

[0083] Table 16 Compressive strength test of simulated wastewater containing Cd for 14 days (unit: Mpa)

[0084]

[0085] Table 17 Compressive strength test of simulated wastewater containing Pb for 28 days (unit: Mpa)

[0086]

[0087] Table 18 Compressive strength test of simulated wastewater containing Cd for 28 days (unit: Mpa)

[0088]

[0089] As shown in Table 10, Group A is the best formula (ternary composite system) of the cementitious material of the present invention; Groups B, C, and D are the compressive strength of the cementitious materials prepared after orthogonal experiments were conducted after eliminating one raw material and obtaining the best formula; Groups E and F are the compressive strengths of other types of cementitious materials. Comparison of A, E, and F shows that the cementitious material of the present invention has excellent mechanical properties and is significantly better than other cementitious materials; comparison of A, B, C, and D shows that the ternary composite system of fly ash, slag, and semi-dry desulfurization ash proposed in the present invention has a good synergistic effect, and the compressive strength is better than the binary system. The principle is: when fly ash and slag are added at the same time, the activity of slag is first stimulated, and the released heat can stimulate fly ash faster, thereby improving the volcanic ash effect of fly ash. In addition, desulfurized ash contains a large amount of SO3, which stimulates the volcanic ash effect. Fly ash undergoes hydration reaction under the stimulation effect of sulfate activity of desulfurized ash. The generated needle-shaped crystal calcium aluminate is cross-linked and filled with other hydration products, which can increase the compressive strength of cementitious materials. At different ages, the strength meets the national standard for concrete.

[0090] It can be seen from Tables 11 to 18 that compared with other groups of cementitious materials, the ternary composite cementitious material A of the present invention has a better performance when using Cd-containing 2+ , Pb 2+ After heavy metal simulated wastewater, the compressive strength exceeds that of cementitious materials of groups B, C, D, E, and F, both in the early stage (3d) and the later stage (28d). The reason is that the ternary system (fly ash, slag, and desulfurization ash) has a good synergistic effect, which can generate a dense cementitious grid to wrap heavy metal ions, and achieve a good solidification effect in a relatively short time. In addition, the hydration products of the cementitious materials are cross-filled together, which can increase the compressive strength and make it meet the C30 standard (30MPa≤fcu) of GB50010-2010 "Code for Design of Concrete Structures", and can be used in many occasions.

[0091] 3.3 Examples of the present invention

[0092] 3.3.1 Examples of wastewater disposal

[0093] Table 19 Components of a wastewater

[0094]

[0095] After the wastewater and the raw materials of the cementitious material are mixed evenly, an alkali activator is added and mixed evenly, and the cementitious material is demolded to form the cementitious material. The heavy metal leaching concentration is tested after curing for 7 days and 28 days. The test results are as follows: at 7 days, Cd 2+ The leaching concentration was 122 μg / L, and the leaching concentration of Pb2+ was 436 μg / L. At 28 days old, the leaching concentration of Cd 2+The leaching concentration is 65μg / L and the Pb2+ leaching concentration is 141μg / L, both of which are far lower than the limit values ​​specified in the national standard GB5085.3-2001 "Hazardous Waste Identification Standard-Leaching Toxicity Identification" (Pb<5mg / L, Cd<1mg / L).

[0096] 3.3.2 Roadbed example

[0097] After the wastewater and raw materials (semi-dry desulfurization ash, slag, fly ash) are evenly mixed, alkali activator is added and mixed to make a cementitious material, which is used to repair potholes in a small section of road. The compressive strength tests were carried out at the ages of 7d and 28d respectively. The results showed that the strength met the C30 standard (30MPa≤fcu) of GB50010-2010 "Code for Design of Concrete Structures".

[0098] For matters not mentioned above, the prior art applies.

[0099] Although some specific embodiments of the present invention have been described in detail through examples, those skilled in the art should understand that the above examples are for illustration only and are not intended to limit the scope of the present invention. Those skilled in the art to which the present invention belongs may make various modifications or supplements to the specific embodiments described or replace them in a similar manner, but they will not deviate from the direction of the present invention or exceed the scope defined by the attached claims. Those skilled in the art should understand that any modifications, equivalent substitutions, improvements, etc. made to the above embodiments based on the technical essence of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a semi-dry desulfurization ash-fly ash-slag composite cementitious material, Features: The raw materials include the following percentages by mass: fly ash + slag: 50%, semi-dry desulfurization ash: 3%~9%, alkali activator 5%~20%, heavy metal-containing wastewater 20.1%~29.5%; the mass ratio of fly ash to slag is 0.4~2.3:1; The preparation method of the cementitious material is as follows: sieve the above-mentioned mass percentages of semi-dry desulfurization ash, slag and fly ash and mix them evenly, then add waste water and alkali activator and stir evenly, pour into a mold, shake, stand, demould and cure to obtain a semi-dry desulfurization ash-fly ash-slag composite cementitious material; Semi-dry desulfurization ash, slag and fly ash shall be passed through a 120-mesh sieve.

2. The method for preparing the semi-dry desulfurization ash-fly ash-slag composite cementitious material according to claim 1, Features: The alkaline activator is NaOH and sodium water glass Na 2 O·nSiO 2 .

3. The preparation method according to claim 1, Features: The modulus of the base activator is 0.5-2.

0.

4. The preparation method according to claim 1, Features: The alkaline activator is NaOH and sodium water glass Na 2 O·nSiO 2 The preparation process of the alkaline activator solution is as follows: weigh sodium hydroxide into a beaker, add an appropriate amount of distilled water and stir to dissolve, add water glass after cooling, stir and let stand to obtain the alkaline activator solution.

5. The preparation method according to claim 1, Features: Cover with plastic wrap and let stand for 24 hours.

6. A semi-dry desulfurization ash-fly ash-slag composite cementitious material prepared by the preparation method according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Integrated method for dry desulfurization and denitrification and cementing material manufacturing

    CN113117483A

  • Alkali-activated concrete prepared from nonferrous metal beneficiation wastewater

    CN113603435A