A self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating and preparation method thereof

Through self-healing fluorine-containing polyurethane oligomer and fluorosilane coupling agent modified micro-nanoparticle composite coating, the problem of wind power blade ice is solved, and efficient and environmentally friendly anti-ice performance and self-repair function are achieved. It is suitable for On the surface of wind power blades, the power generation efficiency and mechanical stability are improved.

CN116987439BActive Publication Date: 2024-12-06HUANENG WEINING WIND POWER GENERATION CO LTD +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310690430.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-12
Publication Date
2024-12-06
Estimated Expiration
2043-06-12

AI Technical Summary

Technical Problem

Wind power blades are prone to freezing in cold areas, resulting in reduced power generation efficiency and mechanical failure. The existing superhydrophobic coatings lack self-repair and long-term deicing functions, making it difficult to meet the environmental protection and construction needs of the wind power field.

Method used

Micro-nanoparticle paste modified with self-healing fluorine-containing polyurethane oligomers, ultraviolet initiators, fluorosilane coupling agents and other additives are combined to form superhydrophobic coatings through ultraviolet light curing, and polysulfur bonds are introduced. To achieve self-healing function.

Benefits of technology

It realizes non-toxic and harmless superhydrophobic coatings, improves anti-ice performance, weather resistance and service life, has good self-repair capabilities, and is suitable for wind power blade surfaces to meet environmental protection and construction needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116987439B_ABST
    Figure CN116987439B_ABST
Patent Text Reader

Abstract

The present invention discloses a self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating and a preparation method thereof. The coating is compounded with self-repairing fluorinated polyurethane oligomer, ultraviolet light initiator, micro-nano particle slurry modified by fluorinated silane coupling agent, pore opening agent, stabilizer, leveling agent and defoaming agent. The coating is non-toxic and safe to use. The coating after coating and curing has a particularly excellent self-repairing function. It also has the advantages of super-hydrophobicity, high adhesion, weather resistance, water resistance, wear resistance, etc. It can be used for wind turbine blade deicing, outdoor wire and cable deicing and other occasions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an anti-icing coating and a preparation method thereof, and in particular to a self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating and a preparation method thereof; and belongs to the technical field of material surface protective coatings. Background Art

[0002] As a clean and renewable energy source, wind energy has been valued by countries around the world. The principle of wind power generation is to use wind power to drive the windmill blades to rotate, and then increase the rotation speed through the speed increaser to drive the generator to generate electricity. However, a large number of wind turbines are installed in cold areas and (or) high-altitude areas, and face the test of freezing environment when operating in winter. The icing of wind turbine blades will reduce the lift of the airfoil, increase the resistance, cause the blade torque to decrease, and affect the power generation efficiency of the wind turbine. At the same time, due to the increase in ice coverage, the mass distribution of the blades is unbalanced, resulting in asymmetric loads, causing mechanical failures and even shutdowns. Therefore, the anti-freezing problem of wind turbines has become a hot spot in the research of wind power technology, and the anti-icing and de-icing problems have also become technical problems that need to be solved urgently in the field of wind power. The anti-icing and de-icing technology of wind turbine blades in cold areas is of great significance to the safe, economical and efficient operation of wind farms and large wind turbines.

[0003] Applying super-hydrophobic coating is the simplest method for anti-icing and de-icing of wind turbine blades. The invention patent with application number 2019109562952 discloses a method for preparing a super-hydrophobic graphene wind turbine blade anti-icing coating material, which first synthesizes a fluorinated acrylate binary copolymer, and then uses an improved Hummers method to prepare graphene oxide, and then uses an alkaline environment to complete a nucleophilic substitution reaction to prepare alkynyl graphene, and finally grafts the fluorinated acrylate copolymer to the surface of graphene oxide to complete the surface modification of the graphene material. This method can increase the surface contact angle of the material, so that the material has a better anti-icing effect, and the wind turbine blades using this coating have the function of anti-icing.

[0004] With the further development of market demand, new wind turbine blade anti-icing coatings need to not only have reliable anti-icing effects, but also be environmentally friendly, easy to construct and have long-lasting deicing properties. Moreover, wind turbine blade anti-icing coatings are mainly applied to the surface of wind turbine blade materials, and preferably have good self-repairing functions. Therefore, the development of new functional materials with good anti-icing effects, self-repairing, anti-scratch, weather resistance and other functions has become the development trend of wind turbine blade anti-icing coatings. Summary of the invention

[0005] One of the purposes of the present invention is to address the above-mentioned problems existing in the prior art and to provide a polyurethane-based super-hydrophobic wind turbine blade surface protective coating with self-repairing ability; the second purpose is to provide a method for preparing the self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating.

[0006] In order to achieve the above object, the present invention adopts the following technical solution:

[0007] The present invention firstly discloses a self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating, which is prepared by compounding 10 parts by weight of a self-repairing fluorine-containing polyurethane oligomer, 0.2-0.8 parts by weight of an ultraviolet light initiator, 3-8 parts by weight of a micro-nano particle slurry modified by a fluorine-containing silane coupling agent, 0.1-0.3 parts by weight of a pore opening agent, 0.1-0.3 parts by weight of a stabilizer, 0.1-0.3 parts by weight of a leveling agent and 0.1-0.3 parts by weight of a defoaming agent.

[0008] Preferably, the preparation method of the aforementioned self-healing fluorinated polyurethane oligomer is as follows: add 100 parts by mass of fluorinated polyether polyol to a four-necked flask equipped with a stirring device, a thermometer and a condenser, then add polyisocyanate at a ratio of -NCO / -OH substance of 1.3 to 1.5, heat to 60 to 90°C, and react for 2 to 4 hours; then add 20 to 50% of the amount of excess isocyanate substance containing polysulfide diol, and continue to react for 1 to 3 hours; finally, add hydroxyl-containing acrylate, continue to react for 1 to 3 hours to react the remaining isocyanate, cool to room temperature, and obtain a self-healing fluorinated polyurethane oligomer.

[0009] The present invention also discloses a method for preparing a self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating as described above, comprising the following steps:

[0010] S1. Preparation of self-healing fluorinated polyurethane oligomers

[0011] In a four-necked flask equipped with a stirring device, a thermometer and a condenser, 100 parts by mass of a fluorinated polyether polyol is added, and then polyisocyanate is added at a ratio of -NCO / -OH of 1.3 to 1.5, and the mixture is heated to 60 to 90° C. and reacted for 2 to 4 hours; then 20 to 50% of a polysulfide bond-containing diol in excess of the isocyanate substance is added, and the reaction is continued for 1 to 3 hours; finally, a hydroxyl-containing acrylate is added, and the reaction is continued for 1 to 3 hours to react the remaining isocyanate, and the mixture is cooled to room temperature to obtain a self-healing fluorinated polyurethane oligomer;

[0012] S2. Preparation of micro-nano particle modified slurry containing silicon-fluorine-silane coupling agent

[0013] A mixed solution of 5 parts by mass of micro-nano particles, 50 parts by mass of ethanol and 0.5-1 parts by mass of a silicon-fluorine silane coupling agent is added to a four-necked flask equipped with a stirring device, a thermometer and a condenser, heated to 50-70° C., and refluxed for 12-24 hours; after cooling to room temperature, the product is transferred to a rotary evaporator, and the ethanol is removed by heating and distillation; a fluorine-containing active diluent is then added, and ultrasonic dispersion is performed for 1-2 hours to obtain a micro-nano particle modified slurry containing a silicon-fluorine silane coupling agent with a solid content of 15-30%;

[0014] S3. Preparation of self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating

[0015] 10 parts by weight of the self-repairing fluorine-containing polyurethane oligomer prepared in step S1 and 3 to 8 parts by weight of the micro-nano particle slurry modified with the silicon-fluorine-containing silane coupling agent prepared in step S2 are mixed evenly, and then 0.2 to 0.8 parts by weight of ultraviolet light initiator, 0.1 to 0.3 parts by weight of pore opening agent, 0.1 to 0.3 parts by weight of stabilizer, 0.1 to 0.3 parts by weight of leveling agent and 0.1 to 0.3 parts by weight of defoaming agent are added thereto, and the mixture is stirred to mix the various additives evenly, and then ultrasonically dispersed for 2 to 4 hours to obtain a self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating.

[0016] Preferably, the aforementioned polysulfide bond-containing diol has the following structural formula:

[0017]

[0018] Wherein, R is selected from H, C1-C 12 One of the alkane groups and benzene rings.

[0019] More preferably, the aforementioned ultraviolet light initiator is one of 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-2-(4-morpholinyl)-1-[4-(methylthio)phenyl]-1-propanone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone, and benzophenone.

[0020] More preferably, the aforementioned silicon-fluorine-containing silane coupling agent is one of heptadecafluorodecyltrimethoxysilane and tridecafluorooctyltriethoxysilane; and the micro-nano particles are one of micro-nano titanium dioxide, micro-nano silicon dioxide and micro-nano kaolin.

[0021] Further preferably, the aforementioned stabilizer is one of 4-benzoyl-2,2,6,6-tetramethylpiperidine, sebacate (2,2,6,6-tetramethylpiperidinyl) ester, tris (1,2,2,6,6-pentamethylpiperidinyl) phosphite, 3,5-di-tert-butyl-4-hydroxybenzyl phosphate monoethyl ester nickel, 2,2-thiobis (4-tert-octylphenol) nickel-n-butylamine, dibutyl dithiocarbamate nickel, salicylate, and benzotriazole.

[0022] Still further preferably, the leveling agent is one of polyorganosiloxane, polyether-modified polyorganosiloxane and fluorine-containing surfactant; and the defoaming agent is an organosilicon defoaming agent.

[0023] More preferably, the polyisocyanate is one of isophorone diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate and lysine diisocyanate.

[0024] More preferably, the hydroxyl-containing acrylate is one of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate, and hydroxypropyl methacrylate; and the fluorine-containing reactive diluent is one of tridecafluorooctyl methacrylate, dodecafluoroheptyl methacrylate, trifluoroethyl methacrylate, and hexafluorobutyl methacrylate.

[0025] The present invention is beneficial in that:

[0026] (1) The self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating system of the present invention does not contain organic solvents and has the advantages of being non-toxic, harmless, safe to use, and environmentally friendly;

[0027] (2) The coating of the present invention can be applied to the surface of the wind turbine blade by conventional means such as spraying, scraping, and roller coating. The use of ultraviolet (UV) curing can further improve the crosslinking degree of the coating, thereby optimizing the anti-icing adhesion, weather resistance, wear resistance, hydrophobic stability and other properties of the super-hydrophobic wind turbine blade surface;

[0028] (3) In the coating system of the present invention, polysulfide bonds are introduced into the molecular chain. When the surface of the material is damaged, self-repair can be achieved by reorganization of the polysulfide bonds, thereby extending the service life of the polyurethane-based superhydrophobic wind turbine blade surface protective coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a diagram showing the self-repairing effect of the coating prepared in Example 1 of the present invention after forming a film on the surface of a wind turbine blade;

[0030] Figure 2 This is a diagram showing the self-repairing effect of the coating prepared in Example 2 of the present invention after forming a film on the surface of a wind turbine blade;

[0031] Figure 3 This is a diagram showing the self-repairing effect of the coating prepared in Example 3 of the present invention after film formation on the surface of a wind turbine blade;

[0032] Figure 4 This is a diagram showing the self-repairing effect of the coating prepared in Comparative Example 1 of the present invention after forming a film on the surface of a wind turbine blade. DETAILED DESCRIPTION

[0033] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0034] Example 1

[0035] The preparation method of the self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating of this embodiment is as follows:

[0036] S1. Preparation of self-healing fluorinated polyurethane oligomers

[0037] In a four-necked flask equipped with a stirring device, a thermometer and a condenser, 100 parts by mass of fluorinated polyether polyol was added, and then 15 parts by mass of isophorone diisocyanate was added, and the mixture was heated to 60°C and reacted for 4 hours; then 10 parts by mass of a polysulfide bond-containing diol having the following structural formula was added, and the reaction was continued for 3 hours; finally, 12 parts of hydroxyethyl acrylate was added, and the reaction was continued for 3 hours, and the mixture was cooled to room temperature to obtain a self-healing fluorinated polyurethane oligomer.

[0038] Among them, the structural formula of the polysulfide diol is:

[0039] S2. Preparation of micro-nanoparticle modified slurry containing fluorinated silane coupling agent

[0040] In a four-necked flask equipped with a stirring device, a thermometer and a condenser, 5 parts by mass of micro-nano TiO2 particles, 50 parts by mass of ethanol and 0.5 parts by mass of a mixed solution of heptadecafluorodecyltrimethoxysilane were added, heated to 50°C, and refluxed for 24 hours; after cooling to room temperature, the product was transferred to a rotary evaporator, and the ethanol was removed by heating and distillation; then 28 parts by mass of tridecafluorooctyl methacrylate was added, and ultrasonic dispersion was performed for 1 hour to obtain a micro-nano particle slurry modified with a silicon-fluorine silane coupling agent having a solid content of 15%.

[0041] S3. Preparation of self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating

[0042] 10 parts by mass of the self-repairing fluorinated polyurethane oligomer prepared in step S1 and 8 parts by mass of the micro-nano particle slurry modified by the fluorinated silane coupling agent prepared in step S2 are mixed evenly, 0.2 parts by mass of 2-hydroxy-2-methyl-1-phenylacetone, 0.1 parts by mass of 4-benzoyl-2,2,6,6-tetramethylpiperidine, 0.1 parts by mass of polyorganosiloxane leveling agent and 0.1 parts by mass of silicone defoaming agent are added, and the mixture is stirred to mix the various additives evenly, and then ultrasonically dispersed for 2 hours to obtain a self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating.

[0043] Example 2

[0044] The preparation method of the self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating of this embodiment is as follows:

[0045] S1. Preparation of self-healing fluorinated polyurethane oligomers

[0046] In a four-necked flask equipped with a stirring device, a thermometer and a condenser, 100 parts by mass of fluorinated polyether polyol was added, and then 18 parts by mass of hexamethylene diisocyanate was added, heated to 80°C, reacted for 3 hours, and cooled to room temperature; then 12 parts by mass of a polysulfide bond-containing diol having the following structural formula was added, and the reaction was continued for 2 hours; finally, 15 parts of hydroxyethyl methacrylate was added, the reaction was continued for 2 hours, and the self-healing fluorinated polyurethane oligomer was obtained.

[0047] Among them, the structural formula of polysulfide diol is:

[0048] S2. Preparation of micro-nanoparticle modified slurry containing fluorinated silane coupling agent

[0049] In a four-necked flask equipped with a stirring device, a thermometer and a condenser, 5 parts by mass of micro-nano silica particles, 50 parts by mass of methanol and 1 part by mass of a mixed solution of tridecafluorooctyltriethoxysilane were added, heated to 60°C, and refluxed for 18 hours; after cooling to room temperature, the product was transferred to a rotary evaporator, and the methanol was removed by heating and distillation; then 15 parts by mass of dodecafluoroheptyl methacrylate were added, and ultrasonic dispersion was performed for 1.5 hours to obtain a micro-nano particle modified slurry of a fluorine-containing silane coupling agent with a solid content of 25%.

[0050] S3. Preparation of self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating

[0051] 10 parts by mass of the self-repairing fluorine-containing polyurethane oligomer prepared in step S1 and 5 parts by mass of the micro-nanoparticle modified slurry of the fluorine-containing silane coupling agent prepared in step S2 are mixed evenly, and 0.5 parts by mass of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 0.2 parts by mass of tris(1,2,2,6,6-pentamethylpiperidinyl)phosphite, 0.2 parts by mass of polyether-modified polysiloxane leveling agent and 0.2 parts by mass of silicone defoaming agent are added, and stirred to mix various additives evenly, and then ultrasonically dispersed for 3 hours to obtain a self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating.

[0052] Example 3

[0053] The preparation method of the self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating of this embodiment is as follows:

[0054] S1. Preparation of self-healing fluorinated polyurethane oligomers

[0055] In a four-necked flask equipped with a stirring device, a thermometer and a condenser, 100 parts by mass of a fluorinated polyether polyol was added, and then 21 parts by mass of lysine diisocyanate was added, heated to 90°C, reacted for 2 hours, and cooled to room temperature; then 14 parts by mass of a polysulfide bond-containing diol having the following structural formula was added, and the reaction was continued for 1 hour; finally, 17 parts of hydroxypropyl methacrylate was added, the reaction was continued for 1 hour, and the self-healing fluorinated polyurethane oligomer was obtained.

[0056] Among them, the structural formula of polysulfide diol is:

[0057] S2. Preparation of micro-nanoparticle modified slurry containing fluorinated silane coupling agent

[0058] In a four-necked flask equipped with a stirring device, a thermometer and a condenser, 5 parts by mass of micro-nano kaolin particles, 50 parts by mass of methanol and 1.5 parts by mass of a mixed solution of tridecafluorooctyltriethoxysilane were added, heated to 90°C, and refluxed for 12 hours; after cooling to room temperature, the product was transferred to a rotary evaporator, and the methanol was removed by heating and distillation; then 11.6 parts by mass of trifluoroethyl methacrylate was added, and ultrasonic dispersion was performed for 2 hours to obtain a micro-nano particle modified slurry of a fluorine-containing silane coupling agent with a solid content of 30%.

[0059] S3. Preparation of self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating

[0060] 10 parts by mass of the self-repairing fluorinated polyurethane oligomer prepared in step S1 and 3 parts by mass of the micro-nanoparticle modified slurry of the fluorinated silane coupling agent prepared in step S2 are mixed evenly, 0.8 parts by mass of 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone, 0.3 parts by mass of 2,2-thiobis(4-tert-octylphenol)nickel-n-butylamine, 0.3 parts by mass of fluorinated surfactant and 0.3 parts by mass of silicone defoamer are added, and the mixture is stirred to mix the various additives evenly, and then ultrasonically dispersed for 4 hours to obtain a self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating.

[0061] Comparative Example 1

[0062] The preparation method of the surface protective coating of this comparative example is as follows:

[0063] (1) Preparation of polyurethane oligomers

[0064] In a four-necked flask equipped with a stirring device, a thermometer and a condenser, 100 parts by mass of polyether polyol and 15 parts by mass of isophorone diisocyanate were added, heated to 60°C and reacted for 4 hours; then 18 parts by mass of hydroxyethyl acrylate were added and the reaction continued for 3 hours, and cooled to room temperature to obtain a polyurethane oligomer.

[0065] (2) Preparation of micro-nano particle / silane coupling agent modified slurry

[0066] In a four-necked flask equipped with a stirring device, a thermometer and a condenser, 5 parts by mass of micro-nano titanium dioxide particles, 50 parts by mass of methanol and 0.5 parts by mass of a mixed solution of γ-methacryloxypropyltrimethoxysilane were added, heated to 50°C, and refluxed for 24 hours; after cooling to room temperature, the product was transferred to a rotary evaporator, and the methanol was removed by heating distillation; 28 parts of dodecyl methacrylate were added, and ultrasonic dispersion was performed for 1 hour to obtain a micro-nano particle / silane coupling agent modified slurry.

[0067] (3) Preparation of anti-icing coating for wind turbine blades

[0068] 10 parts by mass of the self-repairing polyurethane oligomer prepared above and 8 parts by mass of the micro-nano particle / silane coupling agent modified slurry prepared above were mixed evenly, and then 0.2 parts by mass of 2-hydroxy-2-methyl-1-phenylacetone, 0.1 parts by mass of 4-benzoyl-2,2,6,6-tetramethylpiperidine, 0.1 parts by mass of polyorganosiloxane leveling agent and 0.1 parts by mass of silicone defoaming agent were added, stirred to mix various additives evenly, and then ultrasonically dispersed for 2 hours to obtain the anti-icing coating for wind turbine blades.

[0069] Performance Testing

[0070] The coatings of Examples 1 to 3 and Comparative Example 1 were cured under ultraviolet light for 30 seconds and the performance tests were performed. The results were as follows:

[0071]

[0072] Table 1 Test results of Examples 1 to 3 and Comparative Example 1

[0073] It can be seen from the above table that the coating of the present invention has good aging resistance and corrosion resistance, and the anti-icing performance and contact angle are significantly improved compared with comparative example 1. The reason may be that the ultraviolet light curing promotes the fluorine-containing raw materials to enhance the mechanical strength of the coating, while improving the chemical corrosion resistance and aging resistance of the system.

[0074] In addition, the addition of self-healing fluorinated polyurethane oligomers, fluorinated active diluents, and the combined effects of micro-nanoparticles modified with fluorinated silane coupling agents increase the contact angle of the coating after photocuring to more than 150°, greatly reducing the adhesion between the wind turbine blades and ice, and better meeting the anti-icing needs of wind turbine blades.

[0075] It should be particularly noted that the coating of the present invention introduces polysulfide bonds into the molecular chain, so that the coating film obtained by the polyurethane-based super-hydrophobic wind turbine blade surface protective coating has a self-repairing function, thereby improving its service life. Figure 1 to Figure 4 After the coatings of Examples 1 to 3 and Comparative Example 1 were formed into films, they were damaged by the same external force (similar to Figure 4 It can be seen from the figure that in the self-repair effect test, the self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coatings of Examples 1 to 3 have good self-repairing effects and can be repeatedly self-repaired, and small cracks almost disappear; while the coating of Comparative Example 1 has almost no self-repairing effect, and small cracks will not self-heal.

[0076] In summary, the self-healing polyurethane-based super-hydrophobic wind turbine blade surface protective coating produced by the present invention has excellent performance, good system compatibility, fast curing speed under ultraviolet light irradiation, high production efficiency, easy industrialization, and wide application. No toxic solvents are released during the entire process, and it is a non-toxic, pollution-free, and environmentally friendly coating.

[0077] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the above embodiments do not limit the present invention in any form, and any technical solution obtained by equivalent replacement or equivalent transformation falls within the protection scope of the present invention.

Claims

1. A self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating, characterized in that: The self-repairing fluorinated polyurethane oligomer is prepared by compounding 10 parts by weight of a self-repairing fluorinated polyurethane oligomer, 0.2-0.8 parts by weight of an ultraviolet light initiator, 3-8 parts by weight of a micro-nano particle slurry modified by a fluorinated silane coupling agent, 0.1-0.3 parts by weight of a pore-opening agent, 0.1-0.3 parts by weight of a stabilizer, 0.1-0.3 parts by weight of a leveling agent, and 0.1-0.3 parts by weight of a defoaming agent. The preparation method of the self-repairing fluorinated polyurethane oligomer is as follows: 100 parts by weight of a fluorinated polyether polyol is added to a reaction container, and then polyisocyanate is added at a -NCO / -OH substance ratio of 1.3-1.5, and the mixture is heated to 60-90° C. and reacted for 2-4 hours. h; then add 20~50% of the amount of excess isocyanate substance containing polysulfide diol, and continue to react for 1~3h; finally add hydroxyl-containing acrylate, and continue to react for 1~3h to react with the remaining isocyanate, cool to room temperature, and obtain a self-healing fluorinated polyurethane oligomer.

2. The method for preparing a self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating according to claim 1, characterized in that: The steps include: S1. Preparation of self-healing fluorinated polyurethane oligomers Add 100 parts by mass of fluorinated polyether polyol into a reaction container, then add polyisocyanate at a ratio of -NCO / -OH of 1.3 to 1.5, heat to 60 to 90°C, and react for 2 to 4 hours; then add 20 to 50% of the amount of excess isocyanate substance containing polysulfide diol, and continue to react for 1 to 3 hours; finally, add hydroxyl-containing acrylate, continue to react for 1 to 3 hours to react the remaining isocyanate, and cool to room temperature to obtain a self-healing fluorinated polyurethane oligomer; S2. Preparation of micro-nano particle modified slurry containing fluorinated silane coupling agent A mixed solution of 5 parts by mass of micro-nano particles, 50 parts by mass of ethanol and 0.5-1 parts by mass of a fluorine-containing silane coupling agent is added to a reaction container, heated to 50-70° C., and refluxed for 12-24 hours; after cooling to room temperature, the product is transferred to a rotary evaporator, and the ethanol is removed by heating and distillation; a fluorine-containing active diluent is then added, and ultrasonic dispersion is performed for 1-2 hours to obtain a micro-nano particle modified slurry with a solid content of 15-30% of a fluorine-containing silane coupling agent; S3. Preparation of self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating 10 parts by weight of the self-repairing fluorinated polyurethane oligomer prepared in step S1 and 3 to 8 parts by weight of the micro-nano particle slurry modified by the fluorinated silane coupling agent prepared in step S2 are mixed evenly, and then 0.2 to 0.8 parts by weight of an ultraviolet light initiator, 0.1 to 0.3 parts by weight of a pore-opening agent, 0.1 to 0.3 parts by weight of a stabilizer, 0.1 to 0.3 parts by weight of a leveling agent and 0.1 to 0.3 parts by weight of a defoaming agent are added thereto, and the mixture is stirred to uniformly mix the various additives, and then ultrasonically dispersed for 2 to 4 hours to obtain a self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating.

3. The method for preparing a self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating according to claim 2, characterized in that: The structural formula of the polysulfide-bonded diol is as follows: , Wherein, R is selected from H, C1-C 12 One of the alkane groups and benzene rings.

4. The method for preparing a self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating according to claim 2, characterized in that: The ultraviolet light initiator is one of 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-2-(4-morpholinyl)-1-[4-(methylthio)phenyl]-1-propanone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone and benzophenone.

5. The method for preparing a self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating according to claim 2, characterized in that: The fluorine-containing silane coupling agent is one of heptadecafluorodecyltrimethoxysilane and tridecafluorooctyltriethoxysilane; the micro-nano particles are one of micro-nano titanium dioxide, micro-nano silicon dioxide and micro-nano kaolin.

6. The method for preparing a self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating according to claim 2, characterized in that: The stabilizer is one of 4-benzoyl-2,2,6,6-tetramethylpiperidine, sebacic acid (2,2,6,6-tetramethylpiperidinyl) ester, tris (1,2,2,6,6-pentamethylpiperidinyl) phosphite, 3,5-di-tert-butyl-4-hydroxybenzyl phosphate monoethyl ester nickel, 2,2-thiobis (4-tert-octylphenol) nickel-n-butylamine, dibutyl dithiocarbamate nickel, salicylate, and benzotriazole.

7. The method for preparing a self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating according to claim 2, characterized in that: The leveling agent is one of polyorganosiloxane, polyether-modified polyorganosiloxane and fluorine-containing surfactant; and the defoaming agent is an organosilicon defoaming agent.

8. The method for preparing a self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating according to claim 2, characterized in that: The polyisocyanate is one of isophorone diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate and lysine diisocyanate.

9. The method for preparing a self-repairing polyurethane-based super-hydrophobic wind turbine blade surface protective coating according to claim 2, characterized in that: The hydroxyl-containing acrylate is one of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate, and hydroxypropyl methacrylate; the fluorine-containing active diluent is one of tridecafluorooctyl methacrylate, dodecafluoroheptyl methacrylate, trifluoroethyl methacrylate, and hexafluorobutyl methacrylate.