A kind of steel for non-carburizing gear and its manufacturing method
By optimizing chemical composition and process flow, we use medium carbon, high manganese, high sulfur, low aluminum and low nitrogen for carburizing gear steel, combined with NaOH aqueous solution to quench to form full martensite and martensite + bainite structures. , solves the problem that traditional gear steel needs high temperature carburization, improves production efficiency and hardness, and reduces costs.
Patent Information
- Application Number
- CN202310906456.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-24
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-07-24
AI Technical Summary
Traditional steel for gears requires high-temperature carburizing technology, resulting in many production processes, large energy consumption, high cost, and difficulty in improving surface hardness and core toughness at the same time.
Chemical components are C: 0.33-0.39%, Si: 0.10-0.30%, Mn: 1.70-2.00%, Cr: 0.10-0.30%, P: ≤0.015%, S: 0.050-0.070%, Al: 0.008-0.015 %, N: 0.0025-0.0040% steel for carburizing gears can control the morphology and size of the sulfide through the initial refining, refining, vacuum degassing, continuous casting, steel rolling, forging and NaOH aqueous solution quenching processes to achieve the whole horse The formation of innomate and martensite + bainite structures.
The carburizing process with high surface hardness, good wear resistance and moderate core toughness is achieved, reducing production processes and energy consumption and cost.
Smart Images

Figure CN117004884B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of special steel smelting, and particularly relates to a carburizing-free gear steel and a manufacturing method thereof. Background Art
[0002] Traditional gear steel uses low-carbon alloy steel, and the carbon content is generally less than 0.25%. After forging, the gear steel becomes a gear shape. The gear surface first needs to be carburized at high temperature. The thickness of the carburized layer is generally 0.8-1.2mm. After carburizing, the gear must also be quenched + low-temperature tempered to obtain high surface hardness, high wear resistance and fatigue strength, and keep the core of the gear strong and tough after quenching with low-carbon steel, so that it can withstand large impact loads. The gear carburizing process requires the use of a professional carburizing furnace. The carburizing process requires the gear to be heated to a single-phase austenite zone of about 910℃, and kept warm for 6-8 hours under this high temperature environment, so that the active carbon atoms decomposed in the carburizing medium penetrate into the surface of the gear, thereby obtaining a high-carbon area on the surface of the gear, while the core still maintains the original chemical composition. In order to reduce the gear production process, reduce energy consumption, improve production efficiency, and significantly reduce the cost of gear production, the steel of the present invention optimizes the chemical composition and production method of gear steel, and finally realizes the gear steel carburizing-free process. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a carburizing-free gear steel and a manufacturing method thereof in view of the above-mentioned prior art, wherein the steel sulfide A coarse is grade 0 and A fine is grade ≤2.0; the hardness within 1.2 mm from the steel surface reaches above 56 HRC, and the structure in this area is a full martensitic structure; the hardness at 9 mm from the steel surface is 33-37 HRC, and the structure at this position is a martensite + bainite structure, wherein the content of the martensitic structure is 55-65%.
[0004] The technical solution adopted by the present invention to solve the above-mentioned problem is: a carburizing-free gear steel, the chemical composition weight percentage of the steel is C: 0.33-0.39%, Si: 0.10-0.30%, Mn: 1.70-2.00%, Cr: 0.10-0.30%, P: ≤0.015%, S: 0.050-0.070%, Al: 0.008-0.015%, N: 0.0025-0.0040%, and the remainder is Fe and unavoidable impurities.
[0005] The main functions and design basis of each chemical element of the steel of the present invention are:
[0006] C: Carbon is an important element that affects the surface hardness and structure of steel after quenching. A certain content of carbon is conducive to the formation of full martensite structure within 1.2mm from the surface of the steel after quenching, but too high a carbon content will cause more martensite structure to form 9mm from the surface of the steel after quenching, reducing the toughness of the gear core. Therefore, the carbon content selection range is 0.33-0.39%.
[0007] Si: Silicon is added as a deoxidizer during steelmaking and plays a certain deoxidation role. The silicon content is selected in the range of 0.10-0.30%.
[0008] Mn: Adding enough manganese to the steel will help improve the hardness of the area 1.2mm from the steel surface, making this area extremely wear-resistant. However, as the manganese content increases, the martensite content in the gear core area will continue to increase, the bainite content will continue to decrease, and the toughness of the gear core will gradually decrease. The manganese content selection range is Mn: 1.70 ~ 2.00%.
[0009] Cr: Adding chromium to the steel of the present invention can effectively reduce the critical cooling rate of the steel and improve the hardness and strength at 9 mm from the steel surface after quenching, but at the same time it will reduce the plasticity and toughness at this point. Therefore, the chromium content is selected in the range of 0.10-0.30%.
[0010] P: Phosphorus is a harmful element in steel, which increases the cold brittleness of steel and reduces its plasticity. In the present invention, P:≤0.015%.
[0011] S: The surface and core hardness of the steel of the present invention are both high, resulting in poor cutting performance. Since the steel needs to be further refined in the subsequent process, the steel must have good cutting performance. A large amount of sulfur is added to the steel, and the morphology and size of the sulfides in the steel are controlled through the steelmaking, rolling and forging processes, which greatly improves the cutting performance of the steel. The sulfur content of the present invention is selected in the range of 0.050-0.070%.
[0012] Al: Aluminum plays a role in deoxidation and grain refinement in the steel of the present invention. The steel of the present invention does not require high-temperature carburization, so only a small amount of Al and N elements need to be added to the steel to form a small amount of AlN particles to ensure that the grain structure of the steel does not grow during the rolling and forging processes.
[0013] N: Adding a small amount of nitrogen to the steel combines with the Al element to form AlN particles. A small amount of AlN particles can ensure that the grain structure of the steel does not grow during the rolling and forging processes. The increasing amount of AlN in the steel will precipitate in large quantities on the grain boundaries. Although it can play a role in refining the grains of the steel, it reduces the strength of the grain boundaries of the steel. When the steel is quenched with a 10% (by weight) NaOH aqueous solution, the cooling intensity and cooling rate of the quenching process are too large, which easily causes the steel to tear from the relatively weak strength of the grain boundaries. After quenching, a large number of cracks are finally formed on the surface of the steel. Therefore, the selection range of nitrogen in the steel of the present invention is N: 0.0025-0.0040%.
[0014] The above-mentioned carburizing-free gear steel and its manufacturing method include the following process steps:
[0015] 1) The process of primary refining in a converter and refining in a refining furnace is adopted. Ferrosilicon, ferromanganese, ferrochrome and aluminum-iron alloy are added to the refining furnace in the early stage. After refining, the RH vacuum degassing furnace is used for degassing. The molten steel after vacuum degassing is fed into the FeS line. At the same time, the large-sized long strip sulfides are promoted to float to the surface of the molten steel and be adsorbed by the steel slag by the bottom blowing of inert gas. Argon is used in the early stage of the bottom blowing inert gas, and nitrogen is used in the later stage to fine-tune the nitrogen content of the molten steel. The bottom blowing of nitrogen must be after RH vacuum degassing and bottom blowing of argon. The RH vacuum degassing process not only removes the gas hydrogen in the steel, but also reduces the nitrogen content in the steel. When the inert gas argon is blown at the bottom, as the gas argon is constantly disturbed in the molten steel, part of the nitrogen in the molten steel will float up and finally leave the molten steel. Therefore, the nitrogen content in the molten steel must be fine-tuned after RH vacuum degassing and ladle bottom blowing of argon, so as to ensure that the nitrogen content in the steel can be stably controlled within a narrow range of 0.0025-0.0040% after fine-tuning the nitrogen, and ensure the stability of the gas nitrogen content in the molten steel. The diameter of the pores of the porous air bricks at the bottom of the ladle is ≤30um, the number of pores per square millimeter is ≥500, and the diameter of the bubbles is ≤1mm. The molten steel is cast by continuous casting. By reducing the diameter of the pores of the porous air bricks and increasing the number of pores per unit area, smaller pore diameters of the porous air bricks are conducive to producing bubbles with smaller diameters, and denser pores of the porous air bricks are conducive to producing more diffusely distributed bubbles, because the smaller the diameter of the bubbles, the slower the floating speed. A large number of bubbles with slow floating speed and diffuse distribution increase the chance of collision with large-sized long strip sulfides in the molten steel, which is conducive to removing large-sized long strip sulfides in the molten steel.
[0016] 2) The continuous casting billet is heated in a steel rolling heating furnace, with a heating temperature of 1150°C, a starting rolling temperature of 1100°C, a final rolling temperature ≥900°C, and a rolling reduction ratio of 10-15; the high-temperature steel after rolling is hot sheared within the optimal plastic temperature range, and the optimal plastic temperature range of hot shearing is 825-850°C; the hot sheared steel is immediately placed in a forging heating furnace and heated to 1150°C, with a starting forging temperature of 1100°C, a final forging temperature ≥850°C, a forging ratio of 3-5, and forged into a gear shape. In order to ensure the highest efficiency of hot shearing of rolled steel and reduce the deformation of the end of the steel after hot shearing, the hot shearing process of rolled steel needs to be carried out in the optimal plastic temperature range. The method for determining the optimal plastic temperature range is to conduct tests in the austenite temperature range of steel after rolling (below 900°C). Five temperature ranges of 875-900°C, 850-875°C, 825-850°C, 800-825°C, and 775-800°C are selected for testing. By measuring the deformation of the steel section after hot shearing, it is finally determined that the temperature range with the smallest deformation is 825-850°C, which is the optimal plastic temperature range for steel. In order to ensure that the steel sulfide A coarse is level 0 and A fine ≤ level 2.0, on the basis of removing the large-sized long strip sulfides in the steel during the steelmaking process, the A coarse sulfides remaining in the steel are stretched to A fine inclusions through the rolling and forging process. The A coarse sulfides are level 0; in order to ensure that the length of A fine sulfides is less than 436um (A fine ≤ level 2.0), the rolling compression ratio and forging compression ratio cannot be too large to prevent the A fine sulfides from being continuously stretched, the length of A fine exceeds 436um, and the grade of A fine exceeds level 2.0. Therefore, the rolling compression ratio control range is 10-15, and the forging compression ratio control range is 3-5.
[0017] 3) After forging, the high-temperature steel quickly passes through a 10% (by weight) NaOH aqueous solution to cause the surface to cool rapidly. The hardness within 1.2 mm from the steel surface reaches 56 HRC or more, and the structure in this area is a full martensite structure. Since the martensite transformation end temperature Mf of the steel of the present invention is 215°C, the temperature of the NaOH aqueous solution is controlled at 205-215°C to ensure that the area within 1.2 mm from the steel surface is completely transformed into a martensite structure; then immediately enter a 160-170°C insulation furnace and slowly cool to 160-170°C, and keep warm in this temperature range for 2 hours; after the insulation is completed, the hardness at 9 mm from the steel surface is 33-37 HRC, and the structure at this position is a martensite + bainite structure, in which the content of martensite structure is 55-65%; finally, the steel is air-cooled to room temperature after being taken out of the furnace. After forging, the high-temperature steel quickly passes through a 10% (weight) NaOH aqueous solution to cause the surface to cool rapidly. Compared with quenching with clean water, the cooling intensity of the steel is greater and the cooling rate is faster when quenching with NaOH aqueous solution. When quenching with clean water, the temperature range of 500-600°C is in the steam film stage, and a layer of steam film is wrapped on the surface of the steel. The cooling rate is insufficient at this stage, and local soft spots are easily formed on the surface of the steel. The structure at the soft spot is a small amount of bainite + martensite, and a higher hardness full martensitic structure cannot be formed. When 10% (by weight) of the inorganic compound NaOH is added to the clean water, a vapor film is formed on the surface of the steel during the quenching process, and more NaOH crystals are precipitated on the surface of the steel. This layer of solid crystals will produce a slight explosion at 500-600°C and throw out a cloud of crystals, destroying the vapor film on the surface of the steel and breaking and peeling off the iron oxide scale on the surface of the steel. Therefore, after quenching with a 10% (by weight) NaOH aqueous solution, the steel surface has higher hardness and strength. The austenite on the steel surface that quickly passes through the NaOH aqueous solution is successfully transformed into a full martensite structure. The hardness within 1.2mm from the steel surface can reach more than 56HRC, and the structure at this position is a full martensite structure. The temperature of the NaOH aqueous solution after quenching is controlled at 205-215°C, and then immediately put into a 160-170°C holding furnace and slowly cooled to 160-170°C. It is kept in this temperature range for 2 hours and immediately put into a 160-170°C holding furnace to control the cooling intensity and cooling rate of the steel, thereby avoiding the problem of difficult control of the organization during air cooling of the steel. In this cooling process, the organization 9mm away from the steel surface is slowly reduced in temperature, and eventually transforms into a relatively stable martensite + bainite organization. Keeping in the range of 160-170°C for 2 hours and then taking out of the furnace for air cooling can ensure that the steel organization does not undergo any changes, thereby ensuring that the steel organization is martensite (55-65%) + bainite organization, and the hardness of the steel is 33-37HRC.
[0018] Compared with the prior art, the advantages of the present invention are:
[0019] The present invention is directed to a carburizing-free gear steel, which is designed with medium carbon, high manganese, high sulfur, low aluminum and low nitrogen in composition. Through reasonable steelmaking, rolling and forging processes, the morphology and size of sulfides in the steel are effectively controlled, and the cutting performance of the steel is improved; by using a reasonable cooling process and cooling medium, the hardness and structure within 1.2mm and 9mm from the steel surface are effectively controlled, and the gear parts are carburized-free, reducing the gear production process, reducing energy consumption, improving production efficiency, and greatly reducing the production cost of the gear. The carburizing-free gear steel finally produced is characterized in that: the steel sulfide A coarse is level 0, and A fine ≤ level 2.0; the hardness within 1.2mm from the steel surface reaches more than 56HRC, the structure in this area is a full martensitic structure, the hardness at 9mm from the steel surface is 33-37HRC, and the structure at this position is a martensite + bainite structure, wherein the content of the martensitic structure is 55-65%. The gear steel finally produced has high surface hardness and good wear resistance; the core hardness is moderate and the toughness is good. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a metallographic structure diagram of the area within 1.2 mm from the steel surface in Example 1 of the present invention at a magnification of ×500.
[0021] Figure 2 This is a metallographic structure diagram of the area within 1.2 mm from the steel surface in Example 2 of the present invention at a magnification of 500.
[0022] Figure 3 This is a metallographic structure diagram of the area within 9 mm from the steel surface in Example 3 of the present invention at a magnification of ×500.
[0023] Figure 4 This is a metallographic structure diagram of the area within 9 mm from the steel surface in Example 1 of the present invention at a magnification of ×500. DETAILED DESCRIPTION
[0024] The technical solution of the present invention is described in more detail in conjunction with the preferred embodiments of the present invention. However, these embodiments are only descriptions of the preferred implementation methods of the present invention and cannot impose any limitation on the scope of the present invention.
[0025] Example 1 and Example 2:
[0026] The manufacturing method of a non-carburizing gear steel involved in the two embodiments is as follows: 150t converter primary refining → 150t refining → RH furnace vacuum degassing → continuous casting of small square billets (200mm*200mm) → heating and rolling in a steel rolling heating furnace → hot shearing → heating and forging in a forging heating furnace → rapid penetration of 10% (weight) NaOH aqueous solution → entering a holding furnace (170-230°C) and slowly cooling to below 300°C → exiting the furnace and air cooling to room temperature. Two batches of non-carburizing gear steel were manufactured.
[0027] The steelmaking process uses a 150t converter for primary refining and a 150t refining furnace for refining. Ferrosilicon, ferromanganese, ferrochrome and aluminum-iron alloy are added to the refining furnace in the early stage. After refining, the RH vacuum degassing furnace is used for degassing. The molten steel after vacuum degassing is fed into the FeS line. At the same time, the bottom blowing of inert gas promotes the floating of large-sized long strips of sulfides to the surface of the molten steel and is adsorbed by the slag. Argon is used in the early stage of the bottom blowing inert gas, and nitrogen is used in the later stage to fine-tune the nitrogen content of the molten steel. The pore diameter of the porous air brick at the bottom of the ladle is 30um, the number of pores per square millimeter is ≥500, and the bubble diameter is ≤1mm. The molten steel is cast using continuous casting small square billets (200mm*200mm).
[0028] The continuous casting billet is heated in a steel rolling heating furnace, with a heating temperature of 1150°C, a starting rolling temperature of 1100°C, a final rolling temperature of 925°C (Example 1) and 903°C (Example 2), and a rolling reduction ratio of 10.8 (Example 1) and 14.9 (Example 2); the high-temperature steel after rolling is hot sheared within the optimal plastic temperature range, and the hot shearing temperature is 825-850°C; the hot sheared steel is immediately placed in a forging heating furnace and heated to 1150°C, with an initial forging temperature of 1100°C, a final forging temperature of 859°C (Example 1) and 883°C (Example 2), a forging ratio of 3.1 (Example 1) and 4.7 (Example 2), and is forged into a gear shape.
[0029] After forging, the high-temperature steel material quickly passes through a 10% (by weight) NaOH aqueous solution to cause the surface to cool rapidly. The hardness within a region 1.2 mm from the steel surface is 56.6 HRC (Example 1) and 58.1 HRC (Example 2), and the structure at this position is a full martensite structure; the temperature of the NaOH aqueous solution is controlled at 206°C (Example 1) and 213°C (Example 2), and then immediately enters a 161°C (Example 1) and 170°C (Example 2) insulation furnace and slowly cools to 161°C (Example 1) and 170°C (Example 2), and is kept at this temperature for 2 hours. After the insulation is completed, the hardness at a position 9 mm away from the steel surface is 33.8 HRC (Example 1) and 36.2 HRC (Example 2), and the structure at this position is 57% martensite + 43% bainite structure (Example 1) and 64% martensite + 36% bainite structure (Example 2); finally, the steel material is air-cooled to room temperature after being taken out of the furnace.
[0030] The smelting compositions of the steels obtained in Examples 1 and 2 are shown in Table 1.
[0031] Table 1 Melting composition (wt%)
[0032]
[0033] The levels of sulfides in the steels obtained in Examples 1 and 2 are shown in Table 2.
[0034] Table 2
[0035] A thick A thin Example 1 Level 0 Level 1.5 Example 2 Level 0 Level 2.0
[0036] The microstructure and hardness within 1.2 mm from the steel surface obtained in Examples 1 and 2 are shown in Table 3.
[0037] Table 3
[0038] hardness organize Example 1 56.6HRC Full martensitic structure Example 2 58.1HRC Full martensitic structure
[0039] The microstructure and hardness at 9 mm from the steel surface obtained in Examples 1 and 2 are shown in Table 4.
[0040] Table 4
[0041]
[0042] The present invention is aimed at carburizing-free gear steel, and the composition is designed with medium carbon, high manganese, high sulfur, low aluminum and low nitrogen. Through reasonable steelmaking, rolling and forging processes, the morphology and size of sulfides in steel are effectively controlled, and the cutting performance of steel is improved; by using reasonable cooling process and cooling medium, the hardness and structure in the area of 1.2mm and 9mm from the steel surface are effectively controlled, and the carburizing-free process of gear parts is realized, the gear production process is reduced, the energy consumption is reduced, the production efficiency is improved, and the production cost of gears is greatly reduced. A carburizing-free gear steel is finally produced, characterized in that: the steel sulfide A coarse is level 0, and A fine is ≤2.0; the hardness of the area within 1.2mm from the steel surface reaches 56HRC or more, and the structure at this position is a full martensitic structure, and the hardness at 9mm from the steel surface is 33-37HRC, and the structure at this position is a martensite + bainite structure, wherein the content of martensite structure is 55-65%. The gear steel finally produced has high surface hardness and good wear resistance, moderate core hardness and good toughness. The carburizing-free gear steel manufactured by the present invention fills the domestic gap.
[0043] Although the preferred embodiments of the present invention are described in detail above, it should be clearly understood that various modifications and variations are possible for those skilled in the art. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for manufacturing carburizing-free gear steel, characterized in that The chemical composition of the steel is C: 0.33-0.39%, Si: 0.10-0.30%, Mn: 1.70-2.00%, Cr: 0.10-0.30%, P: ≤0.015%, S: 0.050-0.070%, Al: 0.008-0.015%, N: 0.0025-0.0040%, and the balance is Fe and inevitable impurities; the sulfide A coarse of the steel is 0 level, and A fine is ≤2.0 level; the hardness within 1.2mm from the steel surface reaches 56HRC or more, and the structure in this area is a full martensite structure; the hardness at 9mm from the steel surface is 33-37HRC, and the structure at this position is a martensite + bainite structure, wherein the content of the martensite structure is 55-65%; the method comprises the following steps: 1) Use converter for primary refining and refining furnace for refining. In the early stage of the refining furnace, ferrosilicon, ferromanganese, ferrochrome and ferroaluminum alloy are added. After refining, RH vacuum degassing furnace is used for degassing. The molten steel after vacuum degassing is fed into FeS line. At the same time, inert gas is blown from the bottom to promote large-sized long strips of sulfides to float to the surface of the molten steel and be adsorbed by the slag. 2) The continuous casting billet is heated in a steel rolling heating furnace, with a heating temperature of 1150°C, a starting rolling temperature of 1100°C, a final rolling temperature ≥900°C, and a rolling reduction ratio of 10-15; the high-temperature steel after rolling is hot sheared within the optimal plastic temperature range, and the optimal plastic temperature range of hot shearing is 825-850°C; the hot sheared steel is immediately placed in a forging heating furnace and heated to 1150°C, with a starting forging temperature of 1100°C, a final forging temperature ≥850°C, a forging ratio of 3-5, and forged into a gear shape; 3) After forging, the high-temperature steel quickly passes through a 10% NaOH aqueous solution to cause the surface to cool rapidly. The hardness within 1.2mm from the steel surface reaches more than 56HRC, and the structure in this area is a full martensite structure. Then it is immediately put into a 160-170℃ holding furnace and slowly cooled to 160-170℃, and kept in this temperature range for 2 hours; after the end of the holding, the hardness at 9mm from the steel surface is 33-37HRC, and the structure at this position is martensite + bainite, of which the content of martensite is 55-65%; finally, the steel is taken out of the furnace and air-cooled to room temperature.
2. The method for manufacturing carburization-free gear steel according to claim 1, characterized in that: During the smelting process, argon is used in the early stage of bottom blowing inert gas, and nitrogen is used in the later stage to fine-tune the nitrogen content of the molten steel. Bottom blowing of nitrogen must be preceded by RH vacuum degassing and bottom blowing of argon. The RH vacuum degassing process not only removes the gaseous hydrogen in the steel, but also reduces the nitrogen content in the steel; bottom blowing of inert gas argon, as the gaseous argon is constantly disturbed in the molten steel, part of the nitrogen in the molten steel will float up and eventually leave the molten steel.
3. The method for manufacturing carburization-free gear steel according to claim 1, characterized in that: Fine-tuning of nitrogen content in molten steel must be done after RH vacuum degassing and argon blowing from the bottom of the ladle to ensure that the nitrogen content in the steel can be stably controlled within a narrow range of 0.0025-0.0040% after fine-tuning nitrogen, thereby ensuring the stability of the gas nitrogen content in the molten steel.
4. The method for manufacturing carburization-free gear steel according to claim 1, characterized in that: The bottom of the ladle in step 1) is made of porous air-permeable bricks, the pore diameter is ≤30um, the number of pores per square millimeter is ≥500, the bubble diameter is ≤1mm, and the molten steel is cast by continuous casting process.
5. The method for manufacturing carburization-free gear steel according to claim 1, characterized in that: The method for determining the optimal plastic temperature range in the step 2) is to conduct tests in the austenite temperature range of the steel below 900°C after rolling, and select five temperature ranges of 875-900°C, 850-875°C, 825-850°C, 800-825°C, and 775-800°C for testing. By measuring the deformation of the steel section after hot shearing, it is finally determined that the temperature range with the smallest deformation is 825-850°C, which is the optimal plastic temperature range for steel.
Citation Information
Patent Citations
Low-deformation gear steel and manufacturing method thereof
CN102605260A
Low-silicon medium-carbon gear steel suitable for cold forging machining and manufacturing method thereof
CN112981233A
Steel for universal joint cross shaft for cold extrusion and manufacturing method thereof
CN114959442A
Annealing-free cold heading gear steel and manufacturing method thereof
CN114990430A
Steel for gear having excellent dedendum bending fatigue characteristic and facial pressure fatigue characteristic and gear
JP2002121645A