A tropical Burkholderia parasitica and its application in preparing breathable porous materials

The phosphorus elements are degraded through the tropical parabens PTHQX221017, and the proportion of calcium phosphate particles is regulated, which solves the problems of the complexity of the production of existing breathable materials and the difficulty in regulating the pore structure, and realizes efficient and stable preparation of porous materials, which is environmentally friendly and High feasibility.

CN117106632BActive Publication Date: 2024-11-15SOUTH CHINA AGRICULTURAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310881080.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-17
Publication Date
2024-11-15
Estimated Expiration
2043-07-17

AI Technical Summary

Technical Problem

The production process of existing breathable materials is complex, has high risk, high cost, and is difficult to regulate the pore structure. The production of porous materials by microbial fermentation and gases require strict control of microbial growth conditions, making it difficult to achieve stable adjustment of pore size and porosity.

Method used

The PTHQX221017 of tropical parabuckholderia tropica is used to form porous materials by degrading phosphorus elements, and the porosity is adjusted by regulating the size and proportion of calcium phosphate particles. The biologic agent of this bacteria is used to treat phosphorus-containing cement to form deep And controllable breathable pore structure.

Benefits of technology

A porous breathable material with a pore diameter of 20 to 120 μm, a specific surface area of ​​1.25 to 1.4 m2/kg, and a porosity of 2 to 6%. It has a gentle process, simple operation, green and environmentally friendly, and a stable pore structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117106632B_ABST
    Figure CN117106632B_ABST
Patent Text Reader

Abstract

The present invention discloses a tropical paraburkholderia and its application in the preparation of breathable porous materials. The tropical paraburkholderia PTHQX221017 of the present invention has been deposited in the Guangdong Provincial Microbiological Culture Collection Center on April 21, 2023, and its preservation number is: GDMCC No: 63376. It has the ability to solubilize phosphorus, which is used to dissolve and absorb phosphorus elements, and at the same time, it can form a pore structure in the phosphorus-containing material, thereby preparing a porous breathable material. The present invention adjusts the pore size and porosity by regulating the different sizes of calcium phosphate in the material. Calcium phosphates with diameters of 0.10 to 0.28 mm are used to form pores, and calcium phosphates with a diameter of 0.045 mm are used to form connections between the pores. After being treated with PTHQX221017, the pore diameter reaches 20 to 120 μm, and the specific surface area reaches 1.25 to 1.4 m 2 / kg, the porosity reaches 2-6%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of microbial materials, and in particular to a tropical Burkholderia parakholderiae and an application thereof in preparing a breathable porous material. Background Art

[0002] Breathable materials are breathable structural materials with a certain number of pores of varying sizes formed by the gasification reaction of slurry or by mixing corresponding additives such as foam, carbon-containing compounds, aggregates, fine powder, binders or admixtures into the slurry through high temperature or high pressure treatment. They are breathable, water-permeable and light-weight. For example, permeable bricks, as a common breathable material, are a breathable porous structural material made by mixing concrete, river sand, cement and water and adding a water-permeable agent. They are often used as building bricks for paving roadsides to penetrate rainwater and reduce urban waterlogging.

[0003] However, the production process of permeable bricks is complicated, and traditional permeable bricks on the market are generally manufactured by physical means, that is, by pressing to exclude air and form a porous structure. Its production process is highly dangerous and easy to pollute the environment. It requires large equipment and complex raw materials, which is costly and the pore structure is not easy to control. In addition, some chemical methods can also produce gas to form a pore structure, but the equipment used is complex and the reaction conditions are not easy to control. At present, most microorganisms that dissolve inorganic mineral elements and degrade organic matter are mainly used in agriculture and environmental pollution treatment, and other applications are yet to be developed. Some microorganisms can decompose available insoluble substances, absorb nutrients and water, and metabolize to produce gas, thereby forming pores in the material. For example, yeast can decompose nutrients in dough to produce gas, making it loose and porous. However, the preparation of porous materials by microbial fermentation to produce gas generally requires strict control of microbial growth conditions, thereby regulating pore growth, and it is difficult to achieve the adjustment of pore size, porosity, etc., making the material pores unstable. At the same time, each pore is relatively independent and difficult to connect with each other to achieve the effect of ventilation. Summary of the invention

[0004] The purpose of the present invention is to overcome the above-mentioned deficiencies of the prior art and provide a tropical Burkholderia and its application in preparing a breathable porous material.

[0005] The first object of the present invention is to provide a Paraburkholderia tropicala PTHQX221017.

[0006] The second object of the present invention is to provide the use of the tropical Burkholderia thaliana PTHQX221017 in degrading phosphorus and / or preparing porous materials.

[0007] The third object of the present invention is to provide a biological agent.

[0008] The fourth object of the present invention is to provide the use of the biological agent in degrading phosphorus and / or preparing porous materials.

[0009] A fifth object of the present invention is to provide a method for degrading phosphorus.

[0010] A sixth object of the present invention is to provide a method for preparing a porous material.

[0011] The seventh object of the present invention is to provide a porous material prepared by the above preparation method.

[0012] In order to achieve the above object, the present invention is implemented by the following scheme:

[0013] A tropical Paraburkholderia (Paraburkholderia tropica) PTHQX221017, wherein the tropical Paraburkholderia PTHQX221017 has been deposited in Guangdong Provincial Microbiological Culture Collection Center on April 21, 2023, and its preservation number is: GDMCC No: 63376.

[0014] The present invention also claims to protect the use of the tropical Burkholderia PTHQX221017 in degrading phosphorus elements and / or preparing porous materials.

[0015] Based on this, the present invention provides a biological preparation, wherein the biological preparation contains the tropical Burkholderia thaliana PTHQX221017.

[0016] The present invention also provides application of the biological agent in degrading phosphorus element and / or preparing porous materials.

[0017] The present invention also claims a method for degrading phosphorus, which uses the tropical Burkholderia thaliana PTHQX221017 or the biological agent for degradation.

[0018] The present invention also claims a method for preparing a porous material, wherein the phosphorus-containing material is treated with the tropical Burkholderia PTHQX221017 or the biological agent.

[0019] Furthermore, the phosphorus is calcium phosphate.

[0020] Furthermore, the diameter of the calcium phosphate is 0.045-0.28 mm.

[0021] Among them, larger calcium phosphate particles with a diameter of 0.10 to 0.28 mm are used to form pores; smaller calcium phosphate particles with a diameter of 0.045 mm are used to form connections between the pores, playing the role of connecting the pores, which is beneficial for tropical Burkholderia tropicalis PTHQX221017 to enter the interior of the material and ensure the porosity inside the material.

[0022] Furthermore, the phosphorus-containing material is phosphorus-containing cement.

[0023] Furthermore, the preparation method of the phosphorus-containing cement is: mixing cement, calcium phosphate with a diameter of 0.10 to 0.28 mm and water in a weight ratio of 4 to 8: 1 to 2: 2 to 3 to obtain mixed cement 1; then adding calcium phosphate with a diameter of 0.045 mm to obtain mixed cement 2, and the weight of calcium phosphate with a diameter of 0.045 mm in the mixed cement 2 is 0.4 to 0.6%.

[0024] After the mixed cement 2 solidifies, phosphorus-containing cement is obtained.

[0025] Furthermore, the weight ratio of the cement, the calcium phosphate with a diameter of 0.10 to 0.28 mm and water is 5:1:2.

[0026] Furthermore, the weight of calcium phosphate with a diameter of 0.045 mm in the mixed cement 2 is 0.5%.

[0027] Furthermore, the phosphorus-containing cement is treated by soaking in a bacterial solution containing the tropical Burkholderia thaliana PTHQX221017.

[0028] Furthermore, the OD of tropical Burkholderia thaliana PTHQX221017 in the bacterial solution is 600 The value is 0.8~2.

[0029] Furthermore, the OD of tropical Burkholderia thaliana PTHQX221017 in the bacterial solution is 600 The value is 1.

[0030] Furthermore, the ratio of the bacterial liquid to the phosphorus-containing cement is 100-250 mL: 0.5-10 g.

[0031] Furthermore, the ratio of the bacterial liquid to the phosphorus-containing cement is 100 mL: 0.5-1.8 g.

[0032] Furthermore, the conditions for the immersion treatment are 25-37°C and 120-180r constant temperature culture.

[0033] Furthermore, the conditions for the immersion treatment are constant temperature culture at 28°C and 120r.

[0034] The present invention also claims protection for the porous material prepared by the preparation method.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] The present invention discloses a tropical paraburkholderia (Paraburkholderia tropica) PTHQX221017, which has the ability to dissolve phosphorus and is used to dissolve and absorb inorganic phosphorus elements. At the same time, it can make the phosphorus-containing material form a pore structure, thereby preparing a porous breathable material. The present invention can also adjust the pore size and porosity of the porous breathable material by regulating the ratio of calcium phosphate particles of different sizes in the material to form crystals of different sizes combined with water. Among them, larger calcium phosphate particles with a diameter of 0.10 to 0.28 mm are used to form large pores, and fine calcium phosphate particles with a diameter of 0.045 mm are used to form connections between the pores, which is conducive to bacteria entering the interior of the material and ensuring the porosity inside the material. After the cement block containing calcium phosphate particles with diameters of 0.10 to 0.28 mm and 0.045 mm is treated with tropical paraburkholderia PTHQX221017, the pore diameter can reach 20 to 120 μm and the specific surface area can reach 1.25 to 1.4 m 2 / kg, the porosity can reach 2-6%. At the same time, the preparation conditions of the invention are mild, the operation is simple, green and environmentally friendly, and the feasibility is high. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 Diagram for bacterial streak purification.

[0038] Figure 2 It is the phosphate solubilization circle of bacteria. A is the front side of the culture medium, and B is the back side of the culture medium.

[0039] Figure 3 This is a diagram showing the stable phosphorus solubilization effect after multiple generations of transfer plates.

[0040] Figure 4 Phylogenetic tree of Paraburkholderia tropicalis PTHQX221017.

[0041] Figure 5 This is the surface pore condition of cement blocks (containing 0.10mm+0.045mm calcium phosphate particles) that have not been treated with tropical Burkholderia thaliana PTHQX221017.

[0042] Figure 6 This is the surface pore condition of cement blocks (containing 0.28mm+0.045mm calcium phosphate particles) that have not been treated with tropical Burkholderia thaliana PTHQX221017.

[0043] Figure 7 This is the surface pore condition of cement blocks (containing 0.10mm+0.045mm calcium phosphate particles) treated with tropical Burkholderia thaliana PTHQX221017.

[0044] Figure 8 This is the surface pore condition of cement blocks (containing 0.28mm+0.045mm calcium phosphate particles) treated with tropical Burkholderia thaliana PTHQX221017. DETAILED DESCRIPTION

[0045] The present invention is further described in detail below in conjunction with the accompanying drawings and specific examples of the specification. The examples are only used to explain the present invention and are not used to limit the scope of the present invention. The test methods used in the following examples are conventional methods unless otherwise specified; the materials and reagents used are reagents and materials that can be obtained from commercial channels unless otherwise specified.

[0046] Example 1 Isolation and purification of strains and morphological observation

[0047] 1. Experimental Methods

[0048] 1. Dig the rhizosphere soil with roots about 20 cm above the ground under the Bauhinia tree on the campus of South China Agricultural University and store it in a sealed bag. Sieve the soil to remove sand and other debris, accurately weigh 10g of soil, mix it with 100mL of sterile saline, put it into a 250mL conical flask, shake it by hand for 10 minutes, mix it evenly, and obtain a soil suspension. Use a pipette to draw 1mL of soil suspension, add it to 10mL of sterile water, and prepare 10 -1 Then, a series of soil suspensions with gradient concentrations were prepared in the same way, with concentrations of 10 -2 , 10 -3 , 10 -4 , 10 -5 , 10 -6 and 10 -7 .

[0049] Soil microorganisms were separated by dilution and coating method. 100 μL of each gradient diluted soil suspension was taken and coated on the solidified separation medium (solid medium for insoluble inorganic phosphorus). Two plates were coated for each dilution concentration and cultured statically in a 28°C incubator for 5 days. The colonies with phosphate solubilization circles were observed, and the strains with phosphate solubilization circles were separated and purified by plate streaking method. The strains with the largest phosphate solubilization circle and the best growth state were selected from them, and a phosphate solubilizing bacterium PTHQX221017 capable of solubilizing inorganic phosphate was obtained. The samples were stored in Luria-Bertani (LB) liquid medium at 4°C and used as the bacterial solution for inoculation in subsequent experiments.

[0050] The formula of the insoluble inorganic phosphorus solid culture medium is: glucose 10g / L, (NH4)2SO4 0.5g / L, NaCl 0.2g / L, KCl 0.2g / L, MgSO4·7H2O 0.1g / L, FeSO4·7H2O 0.03g / L, MnSO4·4H2O0.03g / L, Ca3(PO4)210.0g / L and agar powder 15g / L, the solvent is distilled water, and the pH is 7.0-7.2.

[0051] 2. (1) Determination of bacterial growth: 100 mL of insoluble inorganic phosphorus liquid medium (without agar powder) was placed in a 250 mL conical flask, and the bacterial solution stored in LB liquid medium at 4°C was inoculated into 100 mL of insoluble inorganic phosphorus liquid medium at a 1% inoculum rate, and the culture was placed in a shaker at a speed of 180 r / min and a temperature of 28°C. After 48 h of culture, the OD of bacterial growth was measured every 24 h. 600 The rotation speed of 120-180r / min can cultivate the phosphate-solubilizing bacteria PTHQX221017 well.

[0052] (2) Qualitative determination of bacterial phosphate solubilization ability: After the strains preserved in LB liquid medium were activated, they were inoculated with a sterile toothpick on a sparingly soluble inorganic phosphorus solid medium and incubated upside down in a 28°C incubator for 10 days (d). The diameter of the phosphate solubilization zone (D1) and colony diameter (D2) were recorded, and the phosphate solubilization index (PSI=D1 / D2) and phosphate solubilization efficiency (PSE=(D1-D2) / D2×100%) were calculated to preliminarily determine the phosphate solubilization ability of each strain.

[0053] (3) Quantitative determination of bacterial phosphate solubilization ability: The strain was prepared into a bacterial suspension (concentration of about 10 9 cell / mL, i.e. wavelength 600nm, OD 600 The value is 1.0), and the inoculation is carried out according to the ratio of bacterial suspension to insoluble inorganic phosphorus liquid culture medium of 1:100, that is, 1 mL of bacterial suspension is inoculated for every 100 mL of culture medium, and repeated 3 times, with the insoluble inorganic phosphorus liquid culture medium without bacteria as the control. The culture was shaken at 28°C and 160r / min. The soluble phosphorus content and pH value in the bacterial liquid were measured 48h after inoculation, and then measured every 24h for 6 times. Take 2mL of culture solution and centrifuge it at 4000r / min for 10min. The effective phosphorus content of the supernatant was determined by molybdenum blue colorimetry. At the same time, the soluble phosphorus amount was calculated according to the phosphorus standard curve, and the pH value of the supernatant was determined.

[0054] 2. Experimental Results

[0055] (1) Figure 1 As shown in FIG. 1 , it is a streaking purification diagram of the phosphate-solubilizing bacteria PTHQX221017. Figure 2 Shown in A and B are the phosphate-solubilizing circle of the phosphate-solubilizing bacteria PTHQX221017. Figure 3 The phosphate-solubilizing effect of the phosphate-solubilizing bacteria PTHQX221017 is stable after multiple generations of transfer.

[0056] (2) The results of bacterial growth are shown in Table 1. At 48 to 192 h, the OD of the phosphate-solubilizing bacteria PTHQX221017 was 600 The value increases over time.

[0057] Table 1 Growth changes of phosphate-solubilizing bacteria PTHQX221017

[0058]

[0059] (3) Qualitative determination results of bacterial phosphate solubilization ability: average colony diameter 0.3 cm, average phosphate solubilization circle diameter 1.1 cm, phosphate solubilization index >3.66, phosphate solubilization efficiency >266%.

[0060] (4) The results of quantitative determination of bacterial phosphorus solubilization ability are shown in Table 2. From 48 to 120 h, the amount of phosphorus solubilized increased with time and then tended to be stable with a pH of 5 to 7.

[0061] Table 2 Phosphate solubilizing ability of phosphate-solubilizing bacteria PTHQX221017

[0062]

[0063] Example 2 Identification of strains

[0064] 1. Experimental Methods

[0065] (1) Observe the colony and strain morphology of the phosphate-solubilizing bacterium PTHQX221017 and perform Gram staining for identification.

[0066] (2) Using the bacterial suspension of phosphate-solubilizing bacteria PTHQX221017 as a template, PCR amplification was performed with the bacterial 16S rRNA universal primers 27F / 1492R to determine the 16S rRNA gene sequence. The primers used were ordered from Shanghai Shenggong Biotechnology Co., Ltd.

[0067] The PCR reaction system (50 μL) was as follows: 2× Taq Master Mix 25 μL, bacterial suspension of phosphate-solubilizing bacteria PTHQX221017 (OD 600 value is 1.0) 2 μL, 2 μL of each primer, and 19 μL of deionized water.

[0068] PCR amplification program: 94°C for 3 min; 94°C for 30 s, 55°C for 30 s, 72°C for 1 min, for a total of 30 cycles; 72°C for 5 min.

[0069] The PCR amplification product was detected by agarose gel electrophoresis to obtain a fragment of about 1000 bp. After sequencing, it was submitted to the Blast database in NCBI for homology comparison. The obtained 16S rRNA nucleotide sequence was compared by BLAST program on NCBI, and the sequence with higher similarity in the database was retrieved. The phosphate-solubilizing bacteria PTHQX221017 was inoculated into LB liquid culture medium to prepare a bacterial solution and stored at 4°C for use.

[0070] 2. Experimental Results

[0071] (1) The colonies of phosphate-solubilizing bacteria PTHQX221017 are round, with smooth, raised, and moist surfaces. The normal diameter is 0.2 to 1 cm, and the maximum can reach about 2.2 cm. It is milky white in the early stage of growth, and turns yellow in the middle after 3 to 4 weeks of maturity and aging, accompanied by mucus production. The Gram staining of phosphate-solubilizing bacteria PTHQX221017 is negative, and the bacteria are short rods. The growth rate is fast, and a phosphate-solubilizing circle can be formed 3 to 5 days after transfer.

[0072] (2) The nucleotide sequence of the 16sRNA of the obtained phosphate-solubilizing bacteria PTHQX221017 is shown in SEQ ID NO: 1. It has a high homology with Paraburkholderia tropica MW406877.1. The comparison results of the Blast database in NCBI show that the similarity is more than 98%. The sequence is compared with the sequences of closely related species in the BLAST results using MAGE11 analysis software to construct a phylogenetic tree. The results are as follows: Figure 4 Combined with the observation results of the phosphate-solubilizing bacteria PTHQX221017 in Example 1, the phosphate-solubilizing bacteria PTHQX221017 was identified as Paraburkholderia tropica.

[0073] The obtained phosphate-solubilizing bacteria PTHQX2210177 was named Paraburkholderia tropicala PTHQX221017, and was deposited in the Guangdong Provincial Microbiological Culture Collection Center on April 21, 2023. Its preservation number is: GDMCC No: 63376, and the preservation address is 5th Floor, Building 59, No. 100 Xianlie Middle Road, Guangzhou.

[0074] Example 3 Method for preparing breathable material using tropical Burkholderia PTHQX221017

[0075] 1. Experimental Methods

[0076] 1. Grind cement ash and calcium phosphate (Ca3(PO4)2 analytically pure) separately, and the cement used is national standard ordinary silicate P.052.5 cement. Then, the calcium phosphate is sieved through three layers of sieves, respectively through 0.28mm (50 mesh sieve) and 0.10mm (160 mesh sieve), to obtain larger calcium phosphate particles with diameters of 0.28mm and 0.10mm, respectively, for forming pores; the above calcium phosphate is then sieved through 0.045mm (350 mesh sieve) to obtain smaller calcium phosphate particles with a diameter of 0.045mm, which are used to form connections between the pores and play a role in connecting the pores.

[0077] 2. Mix cement, 0.28 mm calcium phosphate and water in 4 weight ratios, namely 4:1:2, 5:1:2, 6:2:3 and 8:2:3. After the cement, calcium phosphate and water in each group are mixed evenly, pour them into a grid mold and smooth them, press them into a solidified state, and then get cement blocks. The weight of a single cement block is 0.5-0.6 g and the shape is a cube. Record the time for the cement blocks to air dry and solidify, and select the weight ratio with the shortest solidification time, i.e. 5:1:2, for subsequent experiments.

[0078] 3. Mix cement, larger calcium phosphate and water in a weight ratio of 5:1:2, where the larger calcium phosphate is calcium phosphate particles with a diameter of 0.28 mm and calcium phosphate particles with a diameter of 0.10 mm, and divide them into two experimental groups. Then add 0.5% by weight of smaller calcium phosphate particles with a diameter of 0.045 mm to each experimental group.

[0079] After the cement, calcium phosphate and water in each group are mixed evenly, they are poured into a grid mold and smoothed, and pressed into a solidified state to obtain cement blocks. The weight of a single cement block is 0.5-0.6g and the shape is a cube. After the cement block is air-dried and solidified, it is steam sterilized at 121°C for 20 minutes to obtain a sterilized cement block. The sterilized cement block is placed in sterile water and soaked and shaken to clean the surface of the cement block to obtain a cement block to be fermented.

[0080] 4. Prepare 1L of phosphorus-free insoluble inorganic phosphorus liquid culture medium, sterilize the phosphorus-free insoluble inorganic phosphorus liquid culture medium with steam at 121°C for 20 minutes, and dispense 100mL of each bottle into a 250mL conical flask for later use. Inoculate the tropical Burkholderia parasitica PTHQX221017 of Example 1 into the sterilized phosphorus-free liquid culture medium under a sterile environment, and inoculate 1mL of the bacterial solution (OD 200,000) of Example 1 into each 100mL of phosphorus-free liquid culture medium. 600 value is 1.0), and a liquid culture medium free of phosphorus is obtained after inoculation.

[0081] The formula of the phosphorus-free liquid culture medium is: glucose 10.0 g / L, (NH4)2SO4 0.5 g / L, NaCl 0.2 g / L, KCl 0.2 g / L, MgSO4·7H2O 0.1 g / L, FeSO4·7H2O 0.03 g / L and MnSO4·4H2O0.03 g / L, the solvent is distilled water, and the pH is 7.0-7.4.

[0082] 5. On the basis of the phosphorus-free liquid culture medium obtained after inoculation, a phosphorus-free liquid culture medium without bacteria was set up as a control group. 2 to 3 cement blocks prepared in step 2 were added to each control group, with a weight of 1 to 1.8 g. There were 4 treatments in total in the experimental group (inoculated with bacteria, 0.10 mm + 0.045 mm calcium phosphate particles and 0.28 mm + 0.045 mm calcium phosphate particles were added, respectively) and the control group (not inoculated with bacteria, 0.10 mm + 0.045 mm calcium phosphate particles and 0.28 mm + 0.045 mm calcium phosphate particles were added, respectively), and each treatment was repeated twice. After that, it was placed in an automatic shaker for constant temperature culture. The culture conditions were a temperature of 28°C and a rotation speed of 120r. After one week of culture in the shaker, the OD 600 The value can reach 1.0 to 1.2. Replace the fresh liquid medium without phosphorus every two weeks, and cycle it for two weeks to supplement the nutrients required for the growth of tropical Burkholderia PTHQX221017.

[0083] 6. According to the growth of the strain after transfer and the growth data in the insoluble inorganic phosphorus liquid medium in Example 1, two cycles were set, that is, observation after 4 weeks of cultivation. After 4 weeks of cultivation, the cement block was clamped with tweezers, the surface moisture was blotted, and it was placed under a stereo microscope for observation and photographed. Finally, according to ASTM C150 / C150M-19 "Standard Procedure for Cement Testing", the specific surface area and porosity of the cement were calculated.

[0084] 2. Experimental Results

[0085] As shown in Table 3, when the weight ratio of cement, larger calcium phosphate and water is 5:1:2, the cement setting time is the shortest.

[0086] Table 3 Effect of cement, calcium phosphate and water weight ratio on cement setting time

[0087]

[0088] like Figure 5 and Figure 6 As shown in the figure, the surface of the cement block in the control group is relatively smooth and flat, and there are naturally shallow fine pores, with a pore diameter of about 1 to 5 μm and a specific surface area of ​​about 1.18 to 1.2 m 2 / kg, the porosity is about 0.5-0.6%. Figure 7As shown in the figure, the cement blocks containing 0.1 mm and 0.045 mm calcium phosphate particles and treated with tropical Burkholderia tropicalis PTHQX221017 had significantly larger and deeper pores than the control group, with pore diameters of about 20 to 50 μm and specific surface areas of about 1.25 to 1.28 m 2 / kg, the porosity is about 2-2.5%. Figure 8 As shown in the figure, the cement blocks containing 0.28 mm and 0.045 mm calcium phosphate particles and treated with tropical Burkholderia tropicalis PTHQX221017 have significantly larger and deeper pores than those in the experimental group containing 0.1 mm and 0.045 mm calcium phosphate particles, with pore diameters of about 80 to 120 μm and specific surface areas of about 1.35 to 1.4 m 2 / kg, and the porosity is about 5-6%.

[0089] The above experimental results show that after being treated with tropical Burkholderia thaliana PTHQX221017 in Example 1, deep, dense and size-controllable air-permeable pores can be formed on the surface of the cement block.

[0090] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. For ordinary technicians in this field, other different forms of changes or modifications can be made based on the above descriptions and ideas. It is not necessary and impossible to list all the implementation methods here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A tropical Burkholderia species ( Paraburkholderia tropica )PTHQX221017, It is characterized in that The tropical Burkholderia PTHQX221017 was deposited in the Guangdong Provincial Microbiological Culture Collection Center on April 21, 2023, and its preservation number is: GDMCC No: 63376.

2. Use of the tropical Burkholderia thaliana PTHQX221017 described in claim 1 in degrading phosphorus and / or preparing porous materials.

3. A biological agent, It is characterized in that The biological preparation contains the tropical Burkholderia thaliana PTHQX221017 described in claim 1.

4. Use of the biological agent according to claim 3 in degrading phosphorus and / or preparing porous materials.

5. A method for degrading phosphorus, It is characterized in that Degradation is carried out using the tropical Burkholderia parasitica PTHQX221017 described in claim 1 or the biological preparation described in claim 3.

6. A method for preparing a porous material, It is characterized in that Treat phosphorus-containing materials with the tropical Burkholderia thaliana PTHQX221017 described in claim 1 or the biological agent described in claim 3.

7. The method according to claim 6, It is characterized in that The phosphorus is calcium phosphate.

8. The method according to claim 7, It is characterized in that The diameter of the calcium phosphate is 0.045-0.28 mm.

9. The method according to claim 6, It is characterized in that The phosphorus-containing material is phosphorus-containing cement.

10. The porous material prepared by the method according to any one of claims 6 to 9.