A three-dimensional carbon nanotube material and its preparation method and application

By embedding metallic cobalt and B and N heteroatoms in carbon nanotubes, a three-dimensional carbon nanotube material with high catalytic activity is prepared, which solves the problems of high cost and complicated preparation of precious metal catalysts and achieves electrocatalysis and zinc-air battery performance. The improvement is suitable for large-scale production and application.

CN117142459BActive Publication Date: 2024-10-15NANTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311123428.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-01
Publication Date
2024-10-15
Estimated Expiration
2043-09-01

AI Technical Summary

Technical Problem

In the existing technology, the scarcity and high cost of precious metal platinum-based catalysts hinder the large-scale application of water electrolysis and metal-air batteries, and the preparation method of three-dimensional heteroatom-doped carbon nanotubes is complicated and difficult to achieve large-scale production.

Method used

A simple and controllable method is used to prepare three-dimensional carbon nanotube materials. By embedding metallic cobalt into carbon nanotubes with B and N heteroatoms, its high conductivity and porous structure are used to adjust the electronic structure and active sites of the catalyst. Forming three-dimensional carbon nanotube materials with high catalytic activity.

Benefits of technology

Realized a three-dimensional carbon nanotube material with low price and excellent catalytic performance, which is suitable for electrocatalytic hydrogen evolution reaction, oxygen reduction reaction and rechargeable zinc-air battery, solving the problems of poor electrocatalytic reaction performance and low power density of zinc-air battery , suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117142459B_ABST
    Figure CN117142459B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of nanomaterial preparation and application, and in particular to a three-dimensional carbon nanotube material and its preparation method and application, comprising: firstly grinding a metal cobalt salt, dicyandiamide and boric acid to obtain a uniform mixture, heating the mixture at a high temperature and using the generated gas as a template to form a three-dimensional carbon nanotube material precursor, secondly carbon thermal reduction of the metal ions in the precursor to metal cobalt nanoparticles, and finally obtaining a three-dimensional carbon nanotube material under the catalytic action of metal cobalt. The present invention uses metal cobalt salt, dicyandiamide and boric acid as catalyst precursors, carbon / nitrogen sources and boron sources respectively, and realizes the controllable preparation of three-dimensional carbon materials assembled by metal cobalt embedded in boron and nitrogen co-doped carbon nanotubes; the prepared carbon nanotube material has good electrocatalytic hydrogen evolution reaction, oxygen reduction reaction and rechargeable zinc-air battery performance. The preparation method has the advantages of simple and controllable synthesis process, easy large-scale preparation and low raw material price.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of nano material preparation and application, and in particular to a three-dimensional carbon nanotube material and a preparation method and application thereof. Background Art

[0002] As energy crisis and environmental degradation become more and more serious, it is urgent to develop clean and efficient new energy and energy devices. Water electrolysis and metal-air batteries, as green and environmentally friendly energy conversion and storage devices, are considered to be effective means to solve the above problems. Hydrogen evolution reaction in water electrolysis is a green and environmentally friendly hydrogen production technology that can effectively use intermittent renewable energy (such as wind and solar energy) as a driving force to obtain hydrogen. Oxygen reduction reaction, as a key reaction of metal-air batteries, involves a four-electron transfer process with slow reaction kinetics. In recent years, researchers have designed and synthesized efficient and robust electrocatalysts by regulating the local coordination environment and electronic configuration of catalysts, thereby reducing the catalytic reaction energy barrier and improving the intrinsic catalytic activity of catalysts. At present, precious metal platinum-based materials have outstanding hydrogen evolution reaction and oxygen reduction reaction performance; however, their scarcity and high cost hinder large-scale application. Therefore, there is an urgent need to develop inexpensive non-precious metal-based catalysts with excellent catalytic performance.

[0003] In recent years, non-precious metal catalysts such as transition metal compounds and carbon materials have been widely studied for their high catalytic activity. Among these catalysts, carbon materials with different nanostructures, such as zero-dimensional carbon dots, one-dimensional carbon nanotubes / nanofibers, two-dimensional carbon nanosheets / graphene and three-dimensional carbon materials, have attracted extensive research by researchers due to their advantages of low cost, adjustable physical and chemical properties and good catalytic activity. Among them, carbon nanotubes have a high specific surface area and porous structure, which can expose a large number of catalytic active sites and improve electron transfer and material transport in electrochemical reactions. By doping carbon nanotubes with heteroatoms such as N, B, S, and P, and using the different electronegativity between carbon and heteroatoms, the electronic structure is adjusted to produce more catalytic active sites and improve the intrinsic catalytic activity. Researchers further improved the catalytic activity by co-doping different heteroatoms. In addition, the construction of porous three-dimensional carbon nanotubes can also increase the number of active sites and shorten the ion transmission distance at the electrode-electrolyte interface, thereby improving the catalytic activity. However, the current preparation method of three-dimensional heteroatom-doped carbon nanotubes is relatively complex, and large-scale production faces great challenges.

[0004] In view of the above problems, the present application urgently needs to use a simple and controllable method to prepare a three-dimensional carbon nanotube material with low price and good catalytic performance. By utilizing the advantages of heteroatom doping and its synergistic effect with metals, the excellent conductivity and porous structure of carbon nanotubes, the three-dimensional carbon nanotube material shows good catalytic activity and stability in catalytic reactions. Summary of the invention

[0005] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a three-dimensional carbon nanotube material and a preparation method and application thereof. The raw material reserves are abundant and the price is low. The carbon nanotube material prepared by the present invention has good electrocatalytic hydrogen evolution reaction, oxygen reduction reaction and rechargeable zinc-air battery performance.

[0006] The purpose of the present invention is to provide a method for preparing a three-dimensional carbon nanotube material. The method has a simple preparation process, a wide source of raw materials, and is conducive to industrial production.

[0007] Another object of the present invention is to provide applications of the three-dimensional carbon nanotube material in the fields of electrocatalytic hydrogen evolution reaction, oxygen reduction reaction and rechargeable zinc-air battery.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions:

[0009] A three-dimensional carbon nanotube material comprises a bulk carbon material with a three-dimensional structure and a carbon nanotube co-doped with B and N heteroatoms embedded in metal cobalt.

[0010] Preferably, the mass ratio of metal cobalt to carbon nanotubes in the carbon nanotube material is 0.01:1-0.5:1.

[0011] A method for preparing a three-dimensional carbon nanotube material, the specific steps are as follows:

[0012] Step 1, grinding metal cobalt salt, dicyandiamide and boric acid in a mortar to obtain a uniform mixture;

[0013] Step 2: placing the mixture in a high-temperature furnace under the protection of an inert gas and heating it to a target temperature at a certain heating rate, using the gas generated during the heating process as a template, keeping the temperature for a period of time, and preparing a three-dimensional carbon material precursor;

[0014] Step 3: Continue to heat the three-dimensional carbon material precursor in a high-temperature furnace at a certain heating rate to a target temperature, reduce the metal ions to metal cobalt nanoparticles through carbon thermal reduction, and keep the temperature for a certain period of time to prepare a three-dimensional carbon nanotube material.

[0015] Preferably, in step 1, the mass ratio of the metal cobalt salt to dicyandiamide is 0.01:1-5:1, the mass ratio of dicyandiamide to boric acid is 1:0.01-1:2, and the metal cobalt salt is cobalt chloride or cobalt nitrate.

[0016] Preferably, in step 2, the inert gas is nitrogen or argon, the heating rate is 1-20° C. / min, the heating target temperature is 400-650° C., and the holding time is 0-10 hours.

[0017] Preferably, in step 3, the heating rate is 1-20°C / min, the heating target temperature is 700-1100°C, and the holding time is 0.5-10 hours.

[0018] The present invention also provides an application of the three-dimensional carbon nanotube material obtained by the preparation method in electrocatalytic hydrogen evolution reaction, oxygen reduction reaction and rechargeable zinc-air battery.

[0019] Preferably, the three-dimensional carbon nanotube material is used as a catalyst for an electrocatalytic reaction, or as an air electrode catalyst for a rechargeable zinc-air battery device.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] 1. The three-dimensional carbon nanotube material prepared by the present invention utilizes the synergistic effect between B and N atoms and the high conductivity and porous morphology of the material itself, which can effectively adjust the electronic structure of the catalyst and expose a large number of catalytic sites, and has high intrinsic catalytic activity and material transfer rate.

[0022] 2. The three-dimensional carbon nanotube material prepared by the present invention exhibits good electrocatalytic hydrogen evolution reaction, oxygen reduction reaction and rechargeable zinc-air battery performance, solving the problems of poor electrocatalytic reaction performance and low power density of zinc-air batteries.

[0023] 3. The synthesis process of the three-dimensional carbon nanotube material prepared by the present invention has the advantages of being simple and controllable, easy to operate, and can be prepared in batches, and the required raw materials are cheap and abundant in reserves. It is suitable for large-scale production, can replace precious metals, and accelerate the application process in related fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Optical and scanning electron microscope photographs of the three-dimensional carbon nanotube material prepared in Example 1 of the present invention;

[0025] Figure 2 The product prepared in Example 1 of the present invention is a catalyst, and the hydrogen evolution reaction performance test diagram of the catalyst in a potassium hydroxide solution;

[0026] Figure 3 The product prepared in Example 1 of the present invention is a catalyst, and the oxygen reduction reaction performance test diagram of the catalyst in a potassium hydroxide solution;

[0027] Figure 4 This is a performance test diagram of a zinc-air battery in which the product prepared in Example 1 of the present invention is used as an air electrode catalyst of a rechargeable zinc-air battery;

[0028] Figure 5This is a stability test diagram of a zinc-air battery using the product prepared in Example 1 of the present invention as an air electrode catalyst of a rechargeable zinc-air battery. DETAILED DESCRIPTION

[0029] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings, so that those skilled in the art can better understand the advantages and features of the present invention, thereby making a clearer definition of the protection scope of the present invention. The embodiments described in the present invention are only a part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. Example

[0030] A method for preparing a three-dimensional carbon nanotube material, the specific steps are as follows:

[0031] 0.2 g of cobalt chloride, 1 g of dicyandiamide (C2H4N4) and 0.1 g of boric acid were placed in a mortar, ground thoroughly to form a uniform mixture, and transferred to a magnetic boat.

[0032] The magnetic boat was placed in a tube furnace, and the tube furnace was heated to 500° C. at a heating rate of 5° C. / min in an inert gas nitrogen atmosphere, and calcined for 0.5 h to obtain a three-dimensional carbon nanotube material precursor.

[0033] The three-dimensional carbon nanotube material precursor was further heated to 800° C. at a heating rate of 5° C. / min in a tube furnace and calcined for 2 h to obtain a three-dimensional carbon nanotube material.

[0034] The three-dimensional carbon nanotube material obtained by the above method was tested for the performance of electrocatalytic hydrogen evolution reaction and oxygen reduction reaction in a three-electrode system; the working electrode catalyst in the electrolytic cell was the product of the present invention, the reference electrode and the counter electrode were silver-silver chloride electrode and carbon rod respectively, the electrolyte was 1 mol / L and 0.1 mol / L potassium hydroxide solution respectively, and the electrochemical properties of the product were tested using a Chenhua electrochemical workstation; all electrode potentials in the electrochemical test results have been converted to reversible hydrogen electrode potential (RHE). In addition, the three-dimensional carbon nanotube material was used as an air electrode catalyst for a rechargeable zinc-air battery, and the zinc-air battery was assembled and its performance was tested.

[0035] The morphology, structure and performance of the three-dimensional carbon nanotube material prepared by the above method were studied. Figure 1 The following are optical and scanning electron microscope images of catalyst three-dimensional carbon nanotube materials. Figure 1 It shows that the synthesized three-dimensional carbon nanotube material is in the shape of a three-dimensional block, and is composed of carbon nanotubes embedded with a large amount of metal cobalt.

[0036] like Figure 2 As shown in the figure, the three-dimensional carbon nanotube material shows good hydrogen evolution reaction activity in an alkaline system, and 10 mA cm -2 The overpotential required for the current density is 128mV; Figure 3 As shown, the catalyst also showed good oxygen reduction reaction activity under alkaline conditions, with an onset potential of 0.98 V and a half-wave potential of 0.87 V.

[0037] like Figure 4 As shown, the catalyst was used as an air electrode catalyst for a rechargeable zinc-air battery and showed high zinc-air battery performance with a power density of 186.2 mW cm -2 ;like Figure 5 As shown, the catalyst was used as an air electrode catalyst for a rechargeable zinc-air battery and exhibited high zinc-air battery cycle stability performance, running for 300 hours. Example

[0038] The same as Example 1, except that cobalt nitrate is replaced by cobalt chloride, the hydrogen evolution reaction, oxygen reduction reaction and the performance of the rechargeable zinc-air battery remain basically unchanged. Example

[0039] The same as Example 1, except that the mass of cobalt chloride was changed to 0.1 g, the obtained carbon nanotube material achieved 10 mA cm -2 The overpotential required for the hydrogen evolution reaction current density is 167mV; the material shows good oxygen reduction reaction activity in alkaline medium, with an onset potential of 0.93V and a half-wave potential of 0.80V. Example

[0040] The same as Example 1, except that the mass of cobalt chloride was changed to 0.3 g, the obtained carbon nanotube material achieved 10 mA cm -2 The overpotential required for the hydrogen evolution reaction current density is 145mV; the material shows good oxygen reduction reaction activity in alkaline medium, with an onset potential of 0.95V and a half-wave potential of 0.83V. Example

[0041] The same as Example 1, except that the mass of cobalt chloride was changed to 0.5 g, the obtained carbon nanotube material achieved 10 mA cm -2 The overpotential required for the hydrogen evolution reaction current density is 128mV; the material shows good oxygen reduction reaction activity in alkaline medium, with an onset potential of 0.92V and a half-wave potential of 0.78V. Example

[0042] The same as Example 1, except that the mass of boric acid was changed to 0.05 g, the obtained carbon nanotube material achieved 10 mA cm -2The overpotential required for the hydrogen evolution reaction current density is 143mV; the material shows good oxygen reduction reaction activity in alkaline medium, with an onset potential of 0.94V and a half-wave potential of 0.82V. Example

[0043] The same as Example 1, except that the mass of boric acid was changed to 0.2 g, the obtained carbon nanotube material achieved 10 mA cm -2 The overpotential required for the hydrogen evolution reaction current density is 149 mV; the material shows good oxygen reduction reaction activity in alkaline medium, with an onset potential of 0.92 V and a half-wave potential of 0.79 V. Example

[0044] The same as Example 1, except that the mass of boric acid was changed to 0.5 g, the obtained carbon nanotube material achieved 10 mA cm -2 The overpotential required for the hydrogen evolution reaction current density is 178mV; the material shows good oxygen reduction reaction activity in alkaline medium, with an onset potential of 0.88V and a half-wave potential of 0.75V. Example

[0045] The same as Example 1, except that the calcination temperature in step c) was changed to 900°C, and the obtained carbon nanotube material achieved 10 mA cm -2 The overpotential required for the hydrogen evolution reaction current density is 137mV; the material shows good oxygen reduction reaction activity in alkaline medium, with an onset potential of 0.97V and a half-wave potential of 0.87V.

[0046] Embodiment 10:

[0047] The same as Example 1, except that the calcination temperature in step c) was changed to 1000°C, and the obtained carbon nanotube material achieved 10 mA cm -2 The overpotential required for the hydrogen evolution reaction current density is 156 mV; the material shows good oxygen reduction reaction activity in alkaline medium, with an onset potential of 0.94 V and a half-wave potential of 0.81 V.

[0048] In summary, the present invention realizes the controllable preparation of three-dimensional carbon nanotube materials by a simple method. The catalyst shows a three-dimensional bulk structure composed of a large number of carbon nanotubes, which has abundant transmission channels, is conducive to exposing a large number of catalytic active sites and material transmission, and the three-dimensional carbon nanotube material shows good electrocatalytic and rechargeable zinc-air battery performance.

[0049] The description and practice disclosed in the present invention are easy to think and understand for ordinary technicians in the technical field, and several improvements and modifications can be made without departing from the principles of the present invention. Therefore, modifications or improvements made without departing from the spirit of the present invention should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing a three-dimensional carbon nanotube material, characterized in that: The three-dimensional carbon nanotube material comprises a bulk carbon material with a three-dimensional structure and a carbon nanotube co-doped with B / N heteroatoms embedded with metal cobalt; The mass ratio of metal cobalt to carbon nanotubes in the carbon nanotube material is 0.01:1-0.5:1; The specific steps of its preparation method are as follows: Step 1, grinding metal cobalt salt, dicyandiamide and boric acid in a mortar to obtain a uniform mixture; Step 2: placing the mixture in a high-temperature furnace under the protection of an inert gas and heating it to a target temperature at a certain heating rate, using the gas generated during the heating process as a template, keeping the temperature for a period of time, and preparing a three-dimensional carbon material precursor; Step 3, the three-dimensional carbon material precursor is continuously heated in a high temperature furnace at a certain heating rate to a target temperature, the metal ions are carbon thermally reduced to metal cobalt nanoparticles, and the temperature is kept for a certain period of time to prepare a three-dimensional carbon nanotube material; In step 1, the mass ratio of the metal cobalt salt to dicyandiamide is 0.01:1-5:1, and the mass ratio of dicyandiamide to boric acid is 1:0.01-1:2; the metal cobalt salt is cobalt chloride or cobalt nitrate; In step 2, the inert gas is nitrogen or argon, the heating rate is 1-20°C / min, the heating target temperature is 400-650°C, and the holding time is 0.5-10 hours; In step 3, the heating rate is 1-20°C / min, the heating target temperature is 700-1100°C, and the holding time is 0.5-10 hours.

2. An application of the three-dimensional carbon nanotube material obtained by the preparation method according to claim 1 in electrocatalytic hydrogen evolution reaction, oxygen reduction reaction and rechargeable zinc-air battery, characterized in that: The three-dimensional carbon nanotube material is used as a catalyst for an electrocatalytic reaction, or as an air electrode catalyst for a rechargeable zinc-air battery device.