Antibacterial skin-friendly fabric

By modifying bamboo charcoal powder and silica, antioxidant bamboo charcoal powder and functionalized silica are prepared for weaving antibacterial and skin-friendly fabrics, solving the problems of insufficient antioxidant, static and breathable properties of spandex fabrics and achieving high efficiency The sterilization and mite removal and antistatic effects improve the aging resistance and comfort of the fabric.

CN117166113BActive Publication Date: 2024-12-03SHANXI MIAOSUIBAO SLEEP TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311142266.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-06
Publication Date
2024-12-03
Estimated Expiration
2043-09-06

AI Technical Summary

Technical Problem

Traditional spandex fabrics have poor oxidation resistance, are prone to aging and fracture, and are prone to static electricity to cause bacterial aggregation, insufficient breathable and hygroscopic performance, affecting comfort.

Method used

Using antioxidant bamboo charcoal micro powder and functionalized silica as fillers, the bamboo charcoal micro powder and silica are modified by plasma treatment and composite catalyst to prepare spandex fibers with antioxidant, antibacterial and antistatic properties, and then weave them into Antibacterial and skin-friendly fabric.

Benefits of technology

It improves the anti-aging performance, breathability and hygroscopicity of spandex fibers, enhances the antibacterial and mite removal effect, improves the comfort of wearing, and significantly improves the anti-static properties of the fabric.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117166113B_ABST
    Figure CN117166113B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of fabric preparation, and discloses an antibacterial skin-friendly fabric, wherein the antibacterial skin-friendly fabric is prepared by using antioxidant bamboo charcoal powder and functionalized silica as fillers, and spandex fiber is prepared and then woven; wherein the antioxidant bamboo charcoal powder is prepared by amination of bamboo charcoal powder and grafting 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid; and the functionalized silica is prepared by grafting imidazole-1-acetic acid after surface modification of nano-silicon dioxide. The fabric woven by the present invention has the characteristics of good hygroscopicity, perspiration permeability, soft skin-friendly, and high tensile strength, and has excellent wearing comfort and easy processing performance. The fabric also has excellent bactericidal and mite-removing effect, aging resistance, and antistatic performance, and can play a role in a long-term and stable manner, and has a wide range of application fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fabric preparation, and in particular to an antibacterial skin-friendly fabric. Background Art

[0002] Throughout history, fabrics have always been an indispensable part of human life. They not only determine the comfort and beauty of clothing, but also reflect the progress of science and technology and the development of culture. In the past, fabrics were mostly woven from natural fibers. Today, chemical fiber fabrics also occupy a place. Among them, spandex fabrics have unique high elasticity and softness, making them the best choice for making underwear. However, underwear is in direct contact with the human body and is easily stained with sweat. If it cannot be discharged in time, it will stick to the surface of the skin, affecting comfort. In addition, a humid environment is more likely to cause the breeding of bacteria and mites, thereby affecting the health of the skin. In addition to contact with sweat, long-term friction can also lead to the generation of static electricity, causing clothing to cling to the body and affect the appearance. The presence of static electricity can also easily cause bacteria to gather on the surface of clothing. Therefore, this requires spandex fabrics to have the properties of breathability, moisture absorption, antibacterial and mite removal, and antistatic. Because there are hydrogen bonds in the molecules of spandex fabrics, they are easily oxidized and deformed, so spandex fabrics also need to have antioxidant properties.

[0003] The patent with publication number CN112266462B discloses an aging-resistant elastic fabric and a preparation method thereof. The patent modifies spandex and introduces a polyether polyol starting from pentaerythritol into its structure to enhance the cross-linking degree of the prepared spandex fiber, thereby making the molecular structure of the spandex more stable and improving the aging resistance of the spandex fiber. At the same time, triethylene glycol is added to make the prepared spandex fiber also have excellent elasticity. Although the patent can improve the aging resistance of spandex, it does not have the ability of antibacterial and mite removal and antistatic effect. When used as underwear, it is easy to cause bacteria to accumulate and affect people's health. Summary of the invention

[0004] The purpose of the present invention is to provide an antibacterial and skin-friendly fabric, which solves the following technical problems: (1) the traditional spandex fabric has poor antioxidant properties and the spandex fibers are easily aged and broken after long-term use; (2) the spandex fabric is prone to generate static electricity, which leads to bacterial adhesion and the breeding of mites; (3) the spandex fabric has poor air permeability and moisture absorption properties and is not very comfortable.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] The invention discloses an antibacterial and skin-friendly fabric, which is prepared by weaving spandex fiber with antioxidant bamboo charcoal micropowder and functionalized silica as fillers; the antioxidant bamboo charcoal micropowder is prepared by aminating bamboo charcoal micropowder and then grafting 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid; the functionalized silica is prepared by modifying the surface of nano-silicon dioxide and then grafting imidazole-1-acetic acid.

[0007] Furthermore, the method for preparing the antioxidant bamboo charcoal powder comprises the following steps:

[0008] (1) placing bamboo charcoal powder in a plasma treatment chamber, introducing ammonia gas for 10-15 minutes, and taking out to obtain amination bamboo charcoal powder;

[0009] (2) The aminated bamboo charcoal powder is placed in ethanol, ultrasonically dispersed for 5-10 minutes, and then 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid and a composite catalyst are added. The temperature is raised to 50-70° C. for reaction for 5-8 hours. After filtering, washing, and vacuum drying, antioxidant bamboo charcoal powder is obtained.

[0010] Through the above technical scheme, ammonia is used in a plasma treatment chamber to aminate the surface of bamboo charcoal micropowder. Under the action of a composite catalyst, the amino group on the surface of the bamboo charcoal micropowder reacts with the carboxyl group in the structure of 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid to obtain antioxidant bamboo charcoal micropowder. The surface of the antioxidant bamboo charcoal micropowder is grafted with imine groups, which can make it evenly dispersed in spandex. At the same time, it is also grafted with hindered phenol groups with antioxidant effects, which can reduce the possibility of spandex breaking due to aging during long-term use and extend the service life of spandex. In addition, the antioxidant bamboo charcoal micropowder also has a rich pore structure, can absorb and evaporate a large amount of water, and has a good moisture absorption and perspiration effect. The bamboo quinone factor in its structure has a certain antibacterial and mite-removing effect, which can effectively kill bacteria and mites, and the ingredients are safe and will not cause irritation to the skin.

[0011] Furthermore, in step (1), the power of the plasma processing chamber is 100-150W, and the atmospheric pressure is 2-5Pa.

[0012] Furthermore, in step (2), the composite catalyst is 4-dimethylaminopyridine and dicyclohexylcarbodiimide in a mass ratio of 3-6:1-2.

[0013] Furthermore, the method for preparing the functionalized silica comprises the following steps:

[0014] S1: Place nano-silicon dioxide in deionized water, ultrasonically disperse for 15-20 minutes, add chloroethyl isocyanate and a catalyst, heat to 65-75°C for reaction for 3-5 hours, filter, wash, and vacuum dry to obtain modified silicon dioxide;

[0015] S2: Place the modified silica in deionized water, add imidazole-1-acetic acid and mix well, reflux reaction, cool to room temperature, filter, wash and vacuum dry to obtain functionalized silica.

[0016] Through the above technical scheme, under the action of a catalyst, the surface of silicon dioxide is modified by using the isocyanate group in the structure of chloroethyl isocyanate to obtain modified silicon dioxide, and then the active chlorine on the surface of the modified silicon dioxide reacts with the imidazole group in the structure of imidazole-1-acetic acid to undergo a quaternization reaction to obtain functionalized silicon dioxide. The surface of the functionalized silicon dioxide has active carboxyl groups and can be uniformly dispersed in the matrix of spandex, thereby solving the problem that the functionalized silicon dioxide is easy to agglomerate in the matrix, so that the mechanical properties of the spandex can be enhanced and the tensile strength of the spandex can be improved. The imidazole quaternary ammonium salt formed on the surface of the functionalized silicon dioxide has excellent antibacterial properties and can significantly improve the antibacterial ability and softness of the spandex after being combined with the spandex. Even if the antibacterial substance is used for a long time, it will not precipitate, and it has a long-lasting antibacterial effect. At the same time, an adsorption film can be formed on the surface of the spandex, which is conducive to the dissipation of static electricity, so that the prepared fabric also has excellent antistatic effect, and can prevent bacteria from agglomerating due to static electricity adsorption, which can cause adverse effects on the human body.

[0017] Furthermore, in step S1, the catalyst is any one of stannous octoate and dibutyltin dilaurate.

[0018] Furthermore, in step S2, the reflux reaction temperature is 80-90° C. and the time is 24-48 hours.

[0019] Furthermore, the method for preparing the antibacterial skin-friendly fabric comprises the following steps:

[0020] Step 1: Mix toluene diisocyanate and polytetramethylene glycol, introduce nitrogen, add dibutyltin dilaurate, stir until the mixture is uniform, heat to 45-55°C for reaction for 1-2h, add 1,4-butanediol, continue to heat to 70-80°C for reaction for 2-3h, cool to 40-45°C, add triethylamine, functionalized silica and antioxidant bamboo charcoal powder, react for 1-3h, add deionized water, stir thoroughly and defoam naturally to obtain polyurethane;

[0021] Step 2: adding polyurethane to N,N-dimethylacetamide, stirring and standing to form a spinning solution, controlling the flow rate of the spinning solution and performing wet spinning, adding the spinning solution to a distilled water coagulation bath after passing through a spinneret, and then stretching, drying, and winding to obtain spandex fibers;

[0022] Step 3: After twisting, fixed twisting, warping and weaving, the spandex fiber is put on a weaving machine to obtain the fabric.

[0023] Furthermore, in step 2, the spinning solution flow rate is 0.4-0.8 ml / h.

[0024] Beneficial effects of the present invention:

[0025] The present invention prepares spandex fiber as fillers by preparing antioxidant bamboo charcoal powder and functionalized silica as fillers and weaves the spandex fiber into fabrics. The woven fabrics have the characteristics of good moisture absorption, perspiration permeability, softness and skin-friendliness, high tensile strength, excellent wearing comfort and easy processing performance. The fabrics also have excellent bactericidal and mite-removing effects, aging resistance and antistatic properties, and can play a long-term and stable role, and have a wide range of applications.

[0026] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for describing the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0028] Figure 1 This is the infrared spectrum of the antioxidant bamboo charcoal powder in Example 1 of the present invention;

[0029] Figure 2 This is a thermal gravimetric curve of nano-silica, modified silica, and functionalized silica in Example 1 of the present invention. DETAILED DESCRIPTION

[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Example 1

[0032] 1. Preparation of Antioxidant Bamboo Charcoal Powder

[0033] (1) placing 2 g of bamboo charcoal powder in a plasma treatment chamber with a power of 100 W and an atmospheric pressure of 2 Pa, introducing ammonia gas for 10 min, and taking out to obtain amination bamboo charcoal powder;

[0034] (2) 2 g of amino-modified bamboo charcoal powder was placed in 80 ml of ethanol, and after ultrasonic dispersion for 5 min, 1.5 g of 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid, 0.06 g of dicyclohexylcarbodiimide and 0.02 g of 4-dimethylaminopyridine were added, and the temperature was raised to 50 ° C for reaction for 5 h. After filtering, washing and vacuum drying, antioxidant bamboo charcoal powder was obtained.

[0035] The antioxidant bamboo charcoal powder was characterized by infrared spectroscopy. Figure 1 As shown, 3392cm -1 The absorption peak of nitrogen-hydrogen bond in the imine group appeared at 3245 cm -1 The absorption peak of hydroxyl group appears at 3021cm -1 The absorption peak of the carbon-hydrogen bond in the benzene ring is 2914 cm -1 The absorption peak of the carbon-hydrogen bond in the methyl group is 1716 cm -1 The absorption peak at is the carbon-oxygen double bond in the ester group. The appearance of the absorption peaks of the imine group and the ester group indicates that the amino group on the surface of the amination bamboo charcoal powder reacts with the carboxyl group in the structure of 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid.

[0036] 2. Preparation of functionalized silica

[0037] S1: 1.5 g of nano-silicon dioxide was placed in 100 ml of deionized water, and after ultrasonic dispersion for 15 min, 1 g of chloroethyl isocyanate and 0.1 g of stannous octoate were added, and the temperature was raised to 65 ° C for reaction for 3 h, and then the modified silicon dioxide was obtained after filtering, washing and vacuum drying;

[0038] S2: Place 2 g of modified silica in 150 ml of deionized water, add 1 g of imidazole-1-acetic acid and mix well, heat to 80 ° C and reflux for 24 hours, cool to room temperature, filter, wash and vacuum dry to obtain functionalized silica.

[0039] Nano-silica, modified silica and functionalized silica were characterized by thermogravimetric analysis. Figure 2 It can be seen that the final mass retention rate of nano-silica at a high temperature of 800°C is 98.2%, and the lost part is due to the evaporation of crystalline water in its structure; the final mass retention rate of modified silica is 56.7%, and the lost part is due to the decomposition of chloroethyl isocyanate grafted on its surface; the final mass retention rate of functionalized silica is 37.6%, and the lost part is due to the decomposition of organic matter grafted on the surface of silica.

[0040] 3. Preparation of antibacterial and skin-friendly fabrics

[0041] Step 1: 10 ml toluene diisocyanate and 8 ml polytetramethylene glycol were mixed, nitrogen was introduced, 0.1 g dibutyltin dilaurate was added, and the mixture was stirred until uniformly mixed. The mixture was heated to 45°C for reaction for 1 h, 1 ml 1,4-butanediol was added, the mixture was heated to 70°C for reaction for 2 h, the mixture was cooled to 40°C, 1.5 ml triethylamine, 1.5 g functionalized silica and 2 g antioxidant bamboo charcoal powder were added, the mixture was reacted for 1 h, and 10 ml deionized water was added. The mixture was stirred thoroughly and defoamed naturally to obtain polyurethane.

[0042] Step 2: adding polyurethane to 50 ml of N,N-dimethylacetamide, stirring and standing to form a spinning solution, controlling the spinning solution flow rate to 0.4 ml / h for wet spinning, adding the spinning solution to a distilled water coagulation bath after passing through a spinneret, and then stretching, drying, and winding to obtain spandex fibers;

[0043] Step 3: After twisting, fixed twisting, warping and weaving, the spandex fiber is put on a weaving machine to obtain the fabric.

[0044] Example 2

[0045] Preparation of antibacterial and skin-friendly fabrics

[0046] Step 1: 12 ml toluene diisocyanate and 10 ml polytetramethylene glycol were mixed, nitrogen was introduced, 0.2 g dibutyltin dilaurate was added, and the mixture was stirred until uniformly mixed. The mixture was heated to 50°C for reaction for 1.5 h, 1.5 ml 1,4-butanediol was added, the mixture was heated to 75°C for reaction for 2.5 h, the mixture was cooled to 42°C, 2 ml triethylamine, 2 g functionalized silica and 2.5 g antioxidant bamboo charcoal powder were added, the mixture was reacted for 2 h, and 12 ml deionized water was added. The mixture was stirred thoroughly and defoamed naturally to obtain polyurethane.

[0047] Step 2: adding polyurethane to 60 ml of N,N-dimethylacetamide, stirring and standing to form a spinning solution, controlling the spinning solution flow rate to 0.6 ml / h, and performing wet spinning. After the spinning solution passes through the spinneret, it is added to a distilled water coagulation bath, and then stretched, drawn, dried, and wound to obtain spandex fibers;

[0048] Step 3: After twisting, fixed twisting, warping and weaving, the spandex fiber is put on a weaving machine to obtain the fabric.

[0049] The preparation method of the antioxidant bamboo charcoal powder and the functionalized silicon dioxide is the same as that in Example 1.

[0050] Example 3

[0051] Preparation of antibacterial and skin-friendly fabrics

[0052] Step 1: 15 ml of toluene diisocyanate and 12 ml of polytetramethylene glycol were mixed, nitrogen was introduced, 0.3 g of dibutyltin dilaurate was added, and the mixture was stirred until uniformly mixed. The mixture was heated to 55°C for reaction for 2 h, 2 ml of 1,4-butanediol was added, the mixture was heated to 80°C for reaction for 3 h, the mixture was cooled to 45°C, 2.5 ml of triethylamine, 2.5 g of functionalized silica and 3 g of antioxidant bamboo charcoal powder were added, the mixture was reacted for 3 h, and 15 ml of deionized water was added. The mixture was fully stirred and naturally defoamed to obtain polyurethane.

[0053] Step 2: adding polyurethane to 80 ml of N,N-dimethylacetamide, stirring and standing to form a spinning solution, controlling the spinning solution flow rate to 0.8 ml / h, and performing wet spinning. After the spinning solution passes through the spinneret, it is added to a distilled water coagulation bath, and then stretched, drawn, dried, and wound to obtain spandex fibers;

[0054] Step 3: After twisting, fixed twisting, warping and weaving, the spandex fiber is put on a weaving machine to obtain the fabric.

[0055] The preparation method of the antioxidant bamboo charcoal powder and the functionalized silicon dioxide is the same as that in Example 1.

[0056] Comparative Example 1

[0057] Fabric preparation

[0058] Step 1: Mix 12 ml toluene diisocyanate and 10 ml polytetramethylene glycol, introduce nitrogen, add 0.2 g dibutyltin dilaurate, stir until the mixture is uniform, heat to 50 ° C and react for 1.5 hours, add 1.5 ml 1,4-butanediol, continue to heat to 75 ° C and react for 2.5 hours, cool to 42 ° C, add 2 ml triethylamine and 2 g functionalized silica, react for 2 hours, add 12 ml deionized water, stir well and defoam naturally to obtain polyurethane;

[0059] Step 2: adding polyurethane to 60 ml of N,N-dimethylacetamide, stirring and standing to form a spinning solution, controlling the spinning solution flow rate to 0.6 ml / h, and performing wet spinning. After the spinning solution passes through the spinneret, it is added to a distilled water coagulation bath, and then stretched, drawn, dried, and wound to obtain spandex fibers;

[0060] Step 3: After twisting, fixed twisting, warping and weaving, the spandex fiber is put on a weaving machine to obtain the fabric.

[0061] The preparation method of functionalized silica is the same as that in Example 1.

[0062] Comparative Example 2

[0063] Step 1: 12 ml toluene diisocyanate and 10 ml polytetramethylene glycol were mixed, nitrogen was introduced, 0.2 g dibutyltin dilaurate was added, and the mixture was stirred until uniformly mixed. The mixture was heated to 50°C for reaction for 1.5 h, 1.5 ml 1,4-butanediol was added, the mixture was heated to 75°C for reaction for 2.5 h, the mixture was cooled to 42°C, 2 ml triethylamine and 2.5 g antioxidant bamboo charcoal powder were added, the mixture was reacted for 2 h, and 12 ml deionized water was added. The mixture was fully stirred and naturally defoamed to obtain polyurethane.

[0064] Step 2: adding polyurethane to 60 ml of N,N-dimethylacetamide, stirring and standing to form a spinning solution, controlling the spinning solution flow rate to 0.6 ml / h, and performing wet spinning. After the spinning solution passes through the spinneret, it is added to a distilled water coagulation bath, and then stretched, drawn, dried, and wound to obtain spandex fibers;

[0065] Step 3: After twisting, fixed twisting, warping and weaving, the spandex fiber is put on a weaving machine to obtain the fabric.

[0066] The preparation method of the antioxidant bamboo charcoal powder is the same as that in Example 1.

[0067] Comparative Example 3

[0068] Step 1: Mix 12 ml toluene diisocyanate and 10 ml polytetramethylene glycol, introduce nitrogen, add 0.2 g dibutyltin dilaurate, stir until the mixture is uniform, heat to 50 ° C and react for 1.5 hours, add 1.5 ml 1,4-butanediol, continue to heat to 75 ° C and react for 2.5 hours, cool to 42 ° C and add 2 ml triethylamine, react for 2 hours, add 12 ml deionized water, stir well and defoam naturally to obtain polyurethane;

[0069] Step 2: adding polyurethane to 60 ml of N,N-dimethylacetamide, stirring and standing to form a spinning solution, controlling the spinning solution flow rate to 0.6 ml / h, and performing wet spinning. After the spinning solution passes through the spinneret, it is added to a distilled water coagulation bath, and then stretched, drawn, dried, and wound to obtain spandex fibers;

[0070] Step 3: After twisting, fixed twisting, warping and weaving, the spandex fiber is put on a weaving machine to obtain the fabric.

[0071] Comparative Example 4

[0072] Step 1: 12 ml toluene diisocyanate and 10 ml polytetramethylene glycol were mixed, nitrogen was introduced, 0.2 g dibutyltin dilaurate was added, and the mixture was stirred until uniformly mixed. The mixture was heated to 50°C for reaction for 1.5 h, 1.5 ml 1,4-butanediol was added, the mixture was heated to 75°C for reaction for 2.5 h, the mixture was cooled to 42°C, 2 ml triethylamine, 2 g functionalized silica and 2.5 g bamboo charcoal powder were added, the mixture was reacted for 2 h, and 12 ml deionized water was added. The mixture was stirred thoroughly and defoamed naturally to obtain polyurethane.

[0073] Step 2: adding polyurethane to 60 ml of N,N-dimethylacetamide, stirring and standing to form a spinning solution, controlling the spinning solution flow rate to 0.6 ml / h, and performing wet spinning. After the spinning solution passes through the spinneret, it is added to a distilled water coagulation bath, and then stretched, drawn, dried, and wound to obtain spandex fibers;

[0074] Step 3: After twisting, fixed twisting, warping and weaving, the spandex fiber is put on a weaving machine to obtain the fabric.

[0075] The preparation method of functionalized silica is the same as that in Example 1.

[0076] Comparative Example 5

[0077] Step 1: 12 ml toluene diisocyanate and 10 ml polytetramethylene glycol were mixed, nitrogen was introduced, 0.2 g dibutyltin dilaurate was added, and the mixture was stirred until uniformly mixed, the temperature was raised to 50°C for reaction for 1.5 h, 1.5 ml 1,4-butanediol was added, the temperature was further raised to 75°C for reaction for 2.5 h, the temperature was lowered to 42°C, 2 ml triethylamine, 2 g nano-silicon dioxide and 2.5 g antioxidant bamboo charcoal powder were added, the reaction lasted for 2 h, and 12 ml deionized water was added, the mixture was fully stirred and the polyurethane was obtained after natural defoaming;

[0078] Step 2: adding polyurethane to 60 ml of N,N-dimethylacetamide, stirring and standing to form a spinning solution, controlling the spinning solution flow rate to 0.6 ml / h, and performing wet spinning. After the spinning solution passes through the spinneret, it is added to a distilled water coagulation bath, and then stretched, drawn, dried, and wound to obtain spandex fibers;

[0079] Step 3: After twisting, fixed twisting, warping and weaving, the spandex fiber is put on a weaving machine to obtain the fabric.

[0080] The preparation method of the antioxidant bamboo charcoal powder is the same as that in Example 1.

[0081] Performance Testing

[0082] ① The fabrics prepared in Example 1 to Example 3 and Comparative Example 1 to Comparative Example 5 were made into samples that met the specifications, and the air permeability of the samples was tested with reference to the standard GB / T5453-1997 "Test for Air Permeability of Textile Fabrics"; the moisture absorption performance of the samples was tested with reference to the standard GB / T12704.1-2009 "Test Method for Moisture Permeability of Textile Fabrics Part 1: Moisture Absorption Method"; the resistivity of the surface of the samples was tested using a DRK321 BI I surface resistivity tester to determine its antistatic ability; with reference to the standard GB / T14337-2022 "Test Method for Tensile Properties of Chemical Staple Fibers", the samples and the samples treated at high temperature at 90°C in an aging box for 24 hours were tested for tensile strength using a universal material testing machine to determine their mechanical properties and anti-aging ability. The specific test results are shown in the table below:

[0083]

[0084]

[0085] It can be seen from the above table that the samples prepared in Examples 1 to 3 are at a relatively high level in terms of air permeability, moisture absorption, antistatic, anti-aging and mechanical properties. The sample prepared in Comparative Example 1 does not add antioxidant bamboo charcoal powder, so it is at a relatively low level in terms of anti-aging, air permeability and moisture absorption. The sample prepared in Comparative Example 2 does not add functionalized silica, so the performance in terms of antistatic and tensile strength is very low. The sample prepared in Comparative Example 3 is at a very low level in terms of anti-aging, air permeability, moisture absorption, antistatic and tensile strength. The sample prepared in Comparative Example 4 directly adds bamboo charcoal powder without surface treatment, and the bamboo charcoal powder agglomerates in the matrix, resulting in poor mechanical properties of the fabric, and average air permeability, moisture absorption, antistatic and anti-aging effects. The sample prepared in Comparative Example 5 directly adds nano-silica, and nano-silica also agglomerates in the matrix, resulting in poor mechanical properties of the fabric, and the other effects are also average.

[0086] ② The fabrics prepared in Example 1 to Example 3 and Comparative Example 1 to Comparative Example 5 were cut into samples that met the specifications, and the samples were tested for antibacterial properties according to the standard GB / T20944.3-2008 "Evaluation of Antibacterial Properties of Textiles Part 3: Oscillation Method"; the sample's mite killing activity was tested using the drop method, and the sample was placed on a well cell culture plate, 2 drops of deionized water were dripped into it to soak it, and three mites were placed on it at the same time. An inverted microscope was used for observation, and observation was performed every one minute until all three mites died. The death time was recorded, and three tests were performed on each sample. The experimental results were averaged to determine the mite killing effect of the sample; the specific test results are shown in the following table:

[0087] Antibacterial property / % Mite removal effect / min Example 1 99.2 2 Example 2 99.4 1 Example 3 99.1 1 Comparative Example 1 93.3 10 Comparative Example 2 92.6 4 Comparative Example 3 65.8 >30 Comparative Example 4 88.2 12 Comparative Example 5 86.9 7

[0088] It can be seen from the above table that the samples prepared in Examples 1 to 3 have excellent antibacterial and mite removal effects. The sample prepared in Comparative Example 1 did not add antioxidant bamboo charcoal powder, and only imidazole quaternary ammonium salt played a role, so the antibacterial effect was better but not as good as the example, and the mite removal effect was average. The sample prepared in Comparative Example 2 did not add functionalized silica, and only antioxidant bamboo charcoal powder played a role, and the mite removal effect was better, but the antibacterial effect was average. The sample prepared in Comparative Example 3 did not add antioxidant bamboo charcoal powder nor functionalized silica, so it had almost no antibacterial and mite removal ability. The samples prepared in Comparative Examples 4 and 5 both produced agglomeration in the matrix, so the antibacterial and mite removal properties were at a poor level.

[0089] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0090] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the scope defined by the concept of the invention, they should all fall within the protection scope of the present invention.

Claims

1. An antibacterial skin-friendly fabric, characterized in that: The fabric is made of spandex fiber prepared by using antioxidant bamboo charcoal powder and functionalized silica as fillers and then woven; the antioxidant bamboo charcoal powder is made by aminating bamboo charcoal powder and then grafting 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid; the functionalized silica is made by modifying the surface of nano-silicon dioxide and then grafting imidazole-1-acetic acid; The preparation method of the antioxidant bamboo charcoal powder comprises the following steps: (1) placing the bamboo charcoal powder in a plasma treatment chamber, introducing ammonia gas for 10-15 minutes, and taking out the powder to obtain the amino-treated bamboo charcoal powder; (2) placing the aminated bamboo charcoal powder in ethanol, ultrasonically dispersing it for 5-10 minutes, adding 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid and a composite catalyst, heating it to 50-70°C for reaction for 5-8 hours, filtering, washing, and vacuum drying to obtain antioxidant bamboo charcoal powder; The composite catalyst is 4-dimethylaminopyridine and dicyclohexylcarbodiimide in a mass ratio of 3-6:1-2; The preparation method of the functionalized silica comprises the following steps: S1: Place nano-silicon dioxide in deionized water, ultrasonically disperse for 15-20 minutes, add chloroethyl isocyanate and a catalyst, heat to 65-75°C for reaction for 3-5 hours, filter, wash, and vacuum dry to obtain modified silicon dioxide; S2: placing the modified silica in deionized water, adding imidazole-1-acetic acid and mixing evenly, reflux reaction, cooling to room temperature, filtering, washing, and vacuum drying to obtain functionalized silica; The catalyst is any one of stannous octoate and dibutyltin dilaurate.

2. The antibacterial skin-friendly fabric according to claim 1, characterized in that: In step (1), the power of the plasma processing chamber is 100-150W, and the atmospheric pressure is 2-5Pa.

3. The antibacterial skin-friendly fabric according to claim 1, characterized in that: In step S2, the reflux reaction temperature is 80-90° C. and the time is 24-48 hours.

4. The antibacterial skin-friendly fabric according to claim 1, characterized in that: The method for preparing the antibacterial skin-friendly fabric comprises the following steps: Step 1: Mix toluene diisocyanate and polytetramethylene glycol, introduce nitrogen, add dibutyltin dilaurate, stir until the mixture is uniform, heat to 45-55°C for reaction for 1-2h, add 1,4-butanediol, continue to heat to 70-80°C for reaction for 2-3h, cool to 40-45°C, add triethylamine, functionalized silica and antioxidant bamboo charcoal powder, react for 1-3h, add deionized water, stir thoroughly and defoam naturally to obtain polyurethane; Step 2: adding polyurethane to N,N-dimethylacetamide, stirring and standing to form a spinning solution, controlling the flow rate of the spinning solution and performing wet spinning, adding the spinning solution to a distilled water coagulation bath after passing through a spinneret, and then stretching, drying, and winding to obtain spandex fibers; Step 3: After twisting, fixed twisting, warping and weaving, the spandex fiber is put on a weaving machine to obtain the fabric.

5. The antibacterial skin-friendly fabric according to claim 4, characterized in that: In step 2, the spinning solution flow rate is 0.4-0.8 ml / h.

Citation Information

Patent Citations

  • An aging-resistant elastic fabric and its preparation method

    CN112266462B

  • Method for preparing bamboo charcoal fiber fabric for home textiles

    CN104294402A

  • Anti-aging PC film label material and preparation method thereof

    CN113637313A