A preparation process of modified lithium vanadium fluorophosphate battery positive electrode material
By modifying tetrafluoroethylene-perfluoroalkoxyvinyl ether copolymer, the dense protective layer is formed on the positive electrode material of vanadium fluorophosphate lithium battery, the problems of poor conductivity and short life are solved, and the safety and circulation performance of the battery are improved .
Patent Information
- Application Number
- CN202311270635.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-28
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-09-28
AI Technical Summary
The existing positive electrode materials of vanadium fluorine-vaporate lithium fluorine phosphate battery have poor conductivity, short life, high energy consumption, and there are safety hazards such as melting and explosion risks.
Modified tetrafluoroethylene-perfluoroalkoxyvinyl ether copolymer is used as the radiation substrate, and a dense protective layer is formed through grafting reaction and amidation, which improves the conductivity and cyclic stability of the positive electrode material, and passes through imidazole group. The group increases the reaction site and promotes the transfer of lithium ions.
Form a dense protective layer to reduce the contact between the positive electrode material and the electrolyte, improve safety and cycling performance, extend battery life, and enhance conductivity and stability.
Smart Images

Figure CN117174871B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ions, in particular to a preparation process of a modified lithium vanadium fluorophosphate battery positive electrode material. Background Art
[0002] At present, the mainstream positive raw materials include lithium cobalt oxide, lithium calcium iron phosphate, lithium manganese oxide, nickel cobalt manganese oxide, nickel cobalt aluminum oxide, lithium-rich manganese-based raw materials, etc. Lithium cobalt oxide positive raw materials are mainly used in 3C consumer electronics, lithium calcium iron phosphate is mainly used in power batteries, lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide have small-scale applications in the fields of power batteries and energy storage batteries, lithium manganese oxide is mainly used in combination with other positive raw materials, and lithium-rich manganese-based raw materials are still in the research and development stage. During use, they will encounter the dissolution of positive raw materials and the electrolyte in The surface dissolution of the positive material may even cause fire, explosion and other safety hazards. At the current stage, the most effective way to deal with the above problems is surface coating. The surface coating method can inhibit the interface side reaction between the positive material and the electrolyte, prevent the dissolution of the connecting metal cations, and improve its cycle life. For example, patent CN105226275A reports a modified lithium vanadium fluorophosphate lithium battery positive electrode material and its preparation method, which has good charge and discharge performance, but there is no protective material on the positive electrode surface and the service life is short. Summary of the invention
[0003] 1. Technical issues to be resolved
[0004] In view of the deficiencies in the prior art, the present invention provides a preparation process for a modified lithium vanadium fluorophosphate battery positive electrode material, which solves the problems of poor conductivity, short life and high energy consumption of the lithium vanadium fluorophosphate battery positive electrode material.
[0005] (II) Technical solution
[0006] To achieve the above object, the present invention provides the following technical solution: a preparation process of a modified lithium vanadium fluorophosphate battery positive electrode material, comprising the following process steps:
[0007] (1) 10-20 g of tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer was cut into small pieces of 3 cm × 5 cm, washed with acetone, dried, and stored in an inert atmosphere for irradiation. The irradiation was performed using g-rays generated by Co60 decay at a dose rate of 5-15 kGyh -1 , the irradiated small pieces are stored in a low temperature environment of -26-0°C to obtain a radiated substrate;
[0008] (2) passing nitrogen into the 4-propyleneoxy-2-hydroxybenzophenone monomer for 20-40 minutes to remove oxygen therein, then adding a radiation substrate for grafting reaction, reacting at 40-80° C. for 60-80 hours, filtering, washing and drying to obtain a 4-propyleneoxy-2-hydroxybenzophenone-radiation substrate polymer;
[0009] (3) adding 4-propyleneoxy-2-hydroxybenzophenone-radiation-based polymer to 1,4-dioxane solvent to disperse, adding epichlorohydrin and boron trifluoride ether after uniform dispersion, reacting at 60-100° C. for 6-12 hours, filtering, washing and drying to obtain chlorohydroxy 4-propyleneoxy-2-hydroxybenzophenone-radiation-based polymer;
[0010] (4) adding chlorohydroxy 4-propyleneoxy-2-hydroxybenzophenone-radiation substrate polymer and trimethylamine to N,N-dimethylformamide solvent for amidation reaction, then adding sodium hydroxide solution dropwise to adjust the pH to 7-8, reacting at 50-60° C. for 2-3 hours, and after the reaction is completed, removing the solvent by reduced pressure distillation, filtering, washing with deionized water, and drying to obtain quaternized 4-propyleneoxy-2-hydroxybenzophenone-radiation substrate polymer;
[0011] (5) adding 2,3-diaminobenzoic acid and quaternized 4-propyleneoxy-2-hydroxybenzophenone-radiation base polymer to dimethyl sulfoxide solvent for dissolution, then adding catalyst dibutyltin dilaurate, reacting at 110-140° C. for 15-25 hours, transferring to acetone for washing, filtering and drying to obtain intermediate product A;
[0012] (6) adding the intermediate product A and methyl benzoyl chloride to a toluene solvent, and then adding a catalyst triethanolamine, reacting at 1-5° C. for 2-5 hours, filtering, washing and drying to obtain a modified tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer;
[0013] (7) Add a fluorine source, a phosphorus source, a vanadium source, and a lithium source in a molar ratio of 1:1:1:1 to 15-18 g of a modified tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer, mix the mixture, and then grind the mixture to obtain a powder. The powder is tableted to form an embryo. The embryo is then heated in a heating furnace at 600-800° C. for 8-12 h, and cooled to obtain a modified lithium vanadium fluorophosphate battery positive electrode material.
[0014] Preferably, the weight ratio of 4-propyleneoxy-2-hydroxybenzophenone to the radiation substrate in (2) is 1.2-1.5:1.
[0015] Preferably, the weight ratio of 4-propyleneoxy-2-hydroxybenzophenone-radiation base polymer, epichlorohydrin and boron trifluoride ether in (3) is 1:2-5:0.3-0.5.
[0016] Preferably, the weight ratio of the chlorohydroxy 4-propyleneoxy-2-hydroxybenzophenone-radiation-based polymer to trimethylamine in (4) is 2.1-3.2:1.
[0017] Preferably, the weight ratio of 2,3-diaminobenzoic acid, quaternized 4-propyleneoxy-2-hydroxybenzophenone-radiation-based polymer and catalyst dibutyltin dilaurate in (5) is 1:1.3-2.2:0.2-0.3.
[0018] Preferably, the weight ratio of the intermediate product A, methyl benzoyl chloride and the catalyst triethanolamine in (6) is 1:2.3-2.5:0.3-0.6.
[0019] Preferably, the fluorine source in (7) is one or more of sodium fluoride, ammonium fluoride, and potassium fluoride; the phosphorus source is one or more of ammonium phosphate, potassium dihydrogen phosphate, and sodium dihydrogen phosphate; the vanadium source is vanadium trioxide, vanadium oxalate, and ammonium vanadate; and the lithium source is one or more of lithium acetate, lithium oxalate, lithium carbonate, and lithium hydroxide.
[0020] (III) Beneficial technical effects
[0021] The present invention uses tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer as a radiation substrate, grafts quaternary ammonium salt and positive electrode material, mixes and uniformly distributes on the surface of the positive electrode to form a dense protective layer, delays direct contact between the positive electrode material and the electrolyte, reduces the generation of side reactions, and improves the safety performance and cycle performance of the battery; the quaternized tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer is further reacted with 2,3-diaminobenzoic acid and methyl benzoyl chloride to obtain a tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer containing imidazole groups and quaternary ammonium salt groups, wherein the imidazole groups greatly increase the specific surface area of the positive electrode material, so that the positive electrode material has more reaction sites and accelerates the transfer of lithium ions; the imidazole groups and the quaternary ammonium salt groups synergistically promote the conductivity of the positive electrode and the stability and safety of the cycle. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is the reaction formula of chlorohydroxy 4-propyleneoxy-2-hydroxybenzophenone-radiation substrate polymer.
[0023] Figure 2 It is the reaction formula of modified tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer. DETAILED DESCRIPTION
[0024] Example 1
[0025] (1) 10 g of tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer was cut into small pieces of 3 cm × 5 cm, washed with acetone, dried, and stored in an inert atmosphere for irradiation. The irradiation was performed using g-rays generated by Co60 decay at a dose rate of 5 kGyh -1 , the irradiated small pieces were stored in a low temperature environment of -26°C to obtain the irradiated substrate;
[0026] (2) nitrogen was passed into 4.8 g of 4-propyleneoxy-2-hydroxybenzophenone monomer for 20 min to remove oxygen therein, and then 4 g of irradiated substrate was added for grafting reaction, and the reaction was carried out at 40° C. for 60 h, and the 4-propyleneoxy-2-hydroxybenzophenone-irradiated substrate polymer was obtained by filtering, washing and drying;
[0027] (3) adding 1 g of 4-propyleneoxy-2-hydroxybenzophenone-radiation-based polymer to 1,4-dioxane solvent, dispersing the polymer, adding 2 g of epichlorohydrin and 0.3 g of boron trifluoride ether after the polymer is evenly dispersed, reacting the mixture at 60° C. for 6 h, filtering, washing and drying the mixture to obtain chlorohydroxy 4-propyleneoxy-2-hydroxybenzophenone-radiation-based polymer;
[0028] (4) adding 2.1 g of chlorohydroxy 4-propyleneoxy-2-hydroxybenzophenone-radiation substrate polymer and 1 g of trimethylamine to N,N-dimethylformamide solvent for amidation reaction, then adding sodium hydroxide solution dropwise to adjust the pH to 7, reacting at 50° C. for 2 h, and after the reaction is completed, removing the solvent by reduced pressure distillation, filtering, washing with deionized water, and drying to obtain a quaternized 4-propyleneoxy-2-hydroxybenzophenone-radiation substrate polymer;
[0029] (5) adding 1 g of 2,3-diaminobenzoic acid and 1.3 g of quaternized 4-propyleneoxy-2-hydroxybenzophenone-radiation base polymer to dimethyl sulfoxide solvent for dissolution, then adding 0.2 g of catalyst dibutyltin dilaurate, reacting at 110° C. for 15 h, transferring to acetone for washing, filtering and drying to obtain intermediate product A;
[0030] (6) adding 1 g of the intermediate product A and 2.3 g of methyl benzoyl chloride to a toluene solvent, and then adding 0.3 g of a catalyst triethanolamine, reacting at 1° C. for 2 h, filtering, washing and drying to obtain a modified tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer;
[0031] (7) Sodium fluoride, potassium dihydrogen phosphate, vanadium trioxide, and lithium carbonate were added to 15 g of modified tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer in a molar ratio of 1:1:1:1, and then ground to obtain a powder. The powder was tableted to form an embryo, and the embryo was heated in a heating furnace at 600° C. for 8 h, and cooled to obtain a modified lithium vanadium fluorophosphate battery positive electrode material.
[0032] Example 2
[0033] (1) 20 g of tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer was cut into small pieces of 3 cm × 5 cm, washed with acetone, dried, and stored in an inert atmosphere for irradiation. The irradiation was performed using g-rays generated by Co60 decay at a dose rate of 15 kGyh -1 , the irradiated small pieces are stored in a low temperature environment of 0°C to obtain a radiated substrate;
[0034] (2) nitrogen was passed into 9 g of 4-propyleneoxy-2-hydroxybenzophenone monomer for 40 min to remove oxygen therein, and then 6 g of irradiated substrate was added for grafting reaction, and the reaction was carried out at 80° C. for 80 h, and the 4-propyleneoxy-2-hydroxybenzophenone-irradiated substrate polymer was obtained by filtering, washing and drying;
[0035] (3) adding 1 g of 4-propyleneoxy-2-hydroxybenzophenone-radiation-based polymer to 1,4-dioxane solvent, dispersing the polymer, adding 5 g of epichlorohydrin and 0.5 g of boron trifluoride ether after the polymer is uniformly dispersed, reacting the mixture at 100° C. for 12 h, filtering, washing and drying the mixture to obtain chlorohydroxy 4-propyleneoxy-2-hydroxybenzophenone-radiation-based polymer;
[0036] (4) adding 6.2 g of chlorohydroxy 4-propyleneoxy-2-hydroxybenzophenone-radiation substrate polymer and 1-2 g of trimethylamine to N,N-dimethylformamide solvent for amidation reaction, then adding sodium hydroxide solution dropwise to adjust the pH to 8, reacting at 60° C. for 3 h, and after the reaction is completed, removing the solvent by reduced pressure distillation, filtering, washing with deionized water, and drying to obtain a quaternized 4-propyleneoxy-2-hydroxybenzophenone-radiation substrate polymer;
[0037] (5) adding 3 g of 2,3-diaminobenzoic acid and 6.6 g of quaternized 4-propyleneoxy-2-hydroxybenzophenone-radiation base polymer to dimethyl sulfoxide solvent for dissolution, then adding 0.9 g of catalyst dibutyltin dilaurate, reacting at 140° C. for 25 h, transferring to acetone for washing, filtering and drying to obtain intermediate product A;
[0038] (6) adding 1 g of the intermediate product A and 2.5 g of methyl benzoyl chloride to a toluene solvent, and then adding 0.6 g of a catalyst, triethanolamine, reacting at 5° C. for 5 h, filtering, washing and drying to obtain a modified tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer;
[0039] (7) To 18 g of modified tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer, ammonium fluoride, ammonium phosphate, vanadium trioxide, and lithium hydroxide were added in a molar ratio of 1:1:1:1 and mixed, and then ground to obtain a powder, the powder was tableted to form an embryo, and the embryo was heated in a heating furnace at 800° C. for 12 h, and cooled to obtain a modified lithium vanadium fluorophosphate battery positive electrode material.
[0040] Example 3
[0041] (1) 15 g of tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer was cut into small pieces of 3 cm × 5 cm, washed with acetone, dried, and stored in an inert atmosphere for irradiation. The irradiation was performed using g-rays generated by Co60 decay at a dose rate of 10 kGyh -1 , the irradiated small pieces were stored in a low temperature environment of -13°C to obtain the irradiated substrate;
[0042] (2) nitrogen was passed into 6.9 g of 4-propyleneoxy-2-hydroxybenzophenone monomer for 30 min to remove oxygen therein, and then 5 g of irradiated substrate was added for grafting reaction, and the reaction was carried out at 60° C. for 70 h, and the 4-propyleneoxy-2-hydroxybenzophenone-irradiated substrate polymer was obtained by filtering, washing and drying;
[0043] (3) adding 1 g of 4-propyleneoxy-2-hydroxybenzophenone-radiation-based polymer to 1,4-dioxane solvent to disperse the polymer, adding 3.5 g of epichlorohydrin and 0.4 g of boron trifluoride ether after the polymer is evenly dispersed, reacting at 80° C. for 9 h, filtering, washing and drying to obtain chlorohydroxy 4-propyleneoxy-2-hydroxybenzophenone-radiation-based polymer;
[0044] (4) adding 4.15 g of chlorohydroxy 4-propyleneoxy-2-hydroxybenzophenone-radiation substrate polymer and 1.5 g of trimethylamine to N,N-dimethylformamide solvent for amidation reaction, then adding sodium hydroxide solution dropwise to adjust the pH to 7.5, reacting at 55° C. for 2.5 h, and after the reaction is completed, removing the solvent by reduced pressure distillation, filtering, washing with deionized water, and drying to obtain a quaternized 4-propyleneoxy-2-hydroxybenzophenone-radiation substrate polymer;
[0045] (5) adding 2 g of 2,3-diaminobenzoic acid and 3.95 g of quaternized 4-propyleneoxy-2-hydroxybenzophenone-radiation base polymer to dimethyl sulfoxide solvent for dissolution, then adding 0.55 g of catalyst dibutyltin dilaurate, reacting at 125° C. for 20 h, transferring to acetone for washing, filtering and drying to obtain intermediate product A;
[0046] (6) adding 1 g of the intermediate product A and 2.4 g of methyl benzoyl chloride to a toluene solvent, and then adding 0.45 g of a catalyst triethanolamine, reacting at 3° C. for 3.5 h, filtering, washing and drying to obtain a modified tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer;
[0047] (7) Potassium fluoride, sodium dihydrogen phosphate, ammonium vanadate, and lithium oxalate in a molar ratio of 1:1:1:1 were added to 11.5 g of modified tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer and mixed, and then ground to obtain a powder, the powder was tableted to form an embryo, and the embryo was heated in a heating furnace at 700° C. for 10 h and cooled to obtain a modified lithium vanadium fluorophosphate battery positive electrode material.
[0048] Example 4
[0049] (1) 10 g of tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer was cut into small pieces of 3 cm × 5 cm, washed with acetone, dried, and stored in an inert atmosphere for irradiation. The irradiation was performed using g-rays generated by Co60 decay at a dose rate of 5 kGyh -1 , the irradiated small pieces were stored in a low temperature environment of -26°C to obtain the irradiated substrate;
[0050] (2) nitrogen was passed into 4.8 g of 4-propyleneoxy-2-hydroxybenzophenone monomer for 20 min to remove oxygen therein, and then 4 g of irradiated substrate was added for grafting reaction, and the reaction was carried out at 40° C. for 60 h, and the 4-propyleneoxy-2-hydroxybenzophenone-irradiated substrate polymer was obtained by filtering, washing and drying;
[0051] (3) adding 1 g of 4-propyleneoxy-2-hydroxybenzophenone-radiation-based polymer to 1,4-dioxane solvent, dispersing the polymer, adding 2 g of epichlorohydrin and 0.3 g of boron trifluoride ether after the polymer is evenly dispersed, reacting the mixture at 60° C. for 6 h, filtering, washing and drying the mixture to obtain chlorohydroxy 4-propyleneoxy-2-hydroxybenzophenone-radiation-based polymer;
[0052] (4) adding 6.2 g of chlorohydroxy 4-propyleneoxy-2-hydroxybenzophenone-radiation substrate polymer and 1-2 g of trimethylamine to N,N-dimethylformamide solvent for amidation reaction, then adding sodium hydroxide solution dropwise to adjust the pH to 8, reacting at 50° C. for 2 h, and after the reaction is completed, removing the solvent by reduced pressure distillation, filtering, washing with deionized water, and drying to obtain a quaternized 4-propyleneoxy-2-hydroxybenzophenone-radiation substrate polymer;
[0053] (5) adding 3 g of 2,3-diaminobenzoic acid and 6.6 g of quaternized 4-propyleneoxy-2-hydroxybenzophenone-radiation base polymer to dimethyl sulfoxide solvent for dissolution, then adding 0.9 g of catalyst dibutyltin dilaurate, reacting at 140° C. for 25 h, transferring to acetone for washing, filtering and drying to obtain intermediate product A;
[0054] (6) adding 1 g of the intermediate product A and 2.4 g of methyl benzoyl chloride to a toluene solvent, and then adding 0.45 g of a catalyst triethanolamine, reacting at 3° C. for 3.5 h, filtering, washing and drying to obtain a modified tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer;
[0055] (7) Potassium fluoride, sodium dihydrogen phosphate, ammonium vanadate, and lithium oxalate in a molar ratio of 1:1:1:1 were added to 11.5 g of modified tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer and mixed, and then ground to obtain a powder, the powder was tableted to form an embryo, and the embryo was heated in a heating furnace at 700° C. for 10 h and cooled to obtain a modified lithium vanadium fluorophosphate battery positive electrode material.
[0056] Example 5
[0057] (1) 20 g of tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer was cut into small pieces of 3 cm × 5 cm, washed with acetone, dried, and stored in an inert atmosphere for irradiation. The irradiation was performed using g-rays generated by Co60 decay at a dose rate of 15 kGyh -1 , the irradiated small pieces are stored in a low temperature environment of 0°C to obtain a radiated substrate;
[0058] (2) nitrogen was passed into 9 g of 4-propyleneoxy-2-hydroxybenzophenone monomer for 40 min to remove oxygen therein, and then 6 g of irradiated substrate was added for grafting reaction, and the reaction was carried out at 80° C. for 80 h, and the 4-propyleneoxy-2-hydroxybenzophenone-irradiated substrate polymer was obtained by filtering, washing and drying;
[0059] (3) adding 1 g of 4-propyleneoxy-2-hydroxybenzophenone-radiation-based polymer to 1,4-dioxane solvent, dispersing the polymer, adding 5 g of epichlorohydrin and 0.5 g of boron trifluoride ether after the polymer is uniformly dispersed, reacting the mixture at 100° C. for 12 h, filtering, washing and drying the mixture to obtain chlorohydroxy 4-propyleneoxy-2-hydroxybenzophenone-radiation-based polymer;
[0060] (4) adding 4.15 g of chlorohydroxy 4-propyleneoxy-2-hydroxybenzophenone-radiation substrate polymer and 1.5 g of trimethylamine to N,N-dimethylformamide solvent for amidation reaction, then adding sodium hydroxide solution dropwise to adjust the pH to 7.5, reacting at 60° C. for 3 h, and after the reaction is completed, removing the solvent by reduced pressure distillation, filtering, washing with deionized water, and drying to obtain a quaternized 4-propyleneoxy-2-hydroxybenzophenone-radiation substrate polymer;
[0061] (5) adding 2 g of 2,3-diaminobenzoic acid and 3.95 g of quaternized 4-propyleneoxy-2-hydroxybenzophenone-radiation base polymer to dimethyl sulfoxide solvent for dissolution, then adding 0.55 g of catalyst dibutyltin dilaurate, reacting at 125° C. for 20 h, transferring to acetone for washing, filtering and drying to obtain intermediate product A;
[0062] (6) adding 1 g of the intermediate product A and 2.3 g of methyl benzoyl chloride to a toluene solvent, and then adding 0.3 g of a catalyst triethanolamine, reacting at 1° C. for 2 h, filtering, washing and drying to obtain a modified tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer;
[0063] (7) Sodium fluoride, potassium dihydrogen phosphate, vanadium trioxide, and lithium carbonate were added to 15 g of modified tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer in a molar ratio of 1:1:1:1, and then ground to obtain a powder. The powder was tableted to form an embryo, and the embryo was heated in a heating furnace at 600° C. for 8 h, and cooled to obtain a modified lithium vanadium fluorophosphate battery positive electrode material.
[0064] Comparative Example 1
[0065] (1) Potassium fluoride, sodium dihydrogen phosphate, ammonium vanadate, and lithium oxalate in a molar ratio of 1:1:1:1 are added to a stirrer and mixed, and then ground to obtain a powder, the powder is tableted to form an embryo, and then the embryo is heated in a heating furnace at 700° C. for 10 hours, and cooled to obtain a lithium vanadium fluorophosphate battery positive electrode material.
[0066] The modified lithium vanadium fluorophosphate battery positive electrode material, acetylene black and polyvinylidene fluoride were mixed in a ratio of 6:1:1, N-methylpyrrolidone was added, and after mixing evenly, the mixture was evenly coated on a 6 mm copper foil, and the mixture was placed in an oven for drying to obtain an electrode sheet. A 1 mol / L mixed solution of LiPF6 in ethylene carbonate, dimethyl carbonate and diethyl carbonate was used as the electrolyte. The battery was sealed and allowed to stand for 120 cycles to assemble into a button cell. The initial discharge capacity of the composite electrode material and the discharge capacity after 120 cycles were tested using an IviumStat electrochemical workstation. The test results are shown in Table 1.
[0067] Table 1
[0068]
[0069] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A process for preparing a modified lithium vanadium fluorophosphate battery positive electrode material, characterized in that: The process steps include: (1) 10-20 g of tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer was cut into small pieces of 3 cm × 5 cm, washed with acetone, dried, and stored in an inert atmosphere for irradiation. The irradiation was performed using g-rays generated by Co60 decay at a dose rate of 5-15 kGyh -1 , the irradiated small pieces are stored in a low temperature environment of -26-0°C to obtain a radiated substrate; (2) passing nitrogen into the 4-propyleneoxy-2-hydroxybenzophenone monomer for 20-40 minutes to remove oxygen therein, then adding a radiation substrate for grafting reaction, reacting at 40-80° C. for 60-80 hours, filtering, washing and drying to obtain a 4-propyleneoxy-2-hydroxybenzophenone-radiation substrate polymer; (3) adding 4-propyleneoxy-2-hydroxybenzophenone-radiation-based polymer to 1,4-dioxane solvent to disperse, adding epichlorohydrin and boron trifluoride ether after uniform dispersion, reacting at 60-100° C. for 6-12 hours, filtering, washing and drying to obtain chlorohydroxy 4-propyleneoxy-2-hydroxybenzophenone-radiation-based polymer; (4) adding chlorohydroxy 4-propyleneoxy-2-hydroxybenzophenone-radiation substrate polymer and trimethylamine to N,N-dimethylformamide solvent for amidation reaction, then adding sodium hydroxide solution dropwise to adjust the pH to 7-8, reacting at 50-60° C. for 2-3 hours, and after the reaction is completed, removing the solvent by reduced pressure distillation, filtering, washing with deionized water, and drying to obtain quaternized 4-propyleneoxy-2-hydroxybenzophenone-radiation substrate polymer; (5) adding 2,3-diaminobenzoic acid and quaternized 4-propyleneoxy-2-hydroxybenzophenone-radiation base polymer to dimethyl sulfoxide solvent for dissolution, then adding catalyst dibutyltin dilaurate, reacting at 110-140° C. for 15-25 hours, transferring to acetone for washing, filtering and drying to obtain intermediate product A; (6) adding the intermediate product A and methyl benzoyl chloride to a toluene solvent, and then adding a catalyst triethanolamine, reacting at 1-5° C. for 2-5 hours, filtering, washing and drying to obtain a modified tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer; (7) adding a fluorine source, a phosphorus source, a vanadium source, and a lithium source in a molar ratio of 1:1:1:1 to 15-18 g of a modified tetrafluoroethylene-perfluoroalkoxy vinyl ether copolymer, mixing the mixture, and then grinding the mixture to obtain a powder, pressing the powder into a tablet to form an embryo, and then heating the embryo in a heating furnace at 600-800° C. for 8-12 h, and cooling the embryo to obtain a modified lithium vanadium fluorophosphate battery positive electrode material; The weight ratio of 4-propyleneoxy-2-hydroxybenzophenone to the irradiated substrate in (2) is 1.2-1.5:1; The weight ratio of 4-propyleneoxy-2-hydroxybenzophenone-radiation base polymer, epichlorohydrin and boron trifluoride ether in (3) is 1:2-5:0.3-0.5; The weight ratio of chlorohydroxy 4-propyleneoxy-2-hydroxybenzophenone-radiation base polymer to trimethylamine in (4) is 2.1-3.2:1; The weight ratio of 2,3-diaminobenzoic acid, quaternized 4-propyleneoxy-2-hydroxybenzophenone-radiation-based polymer and catalyst dibutyltin dilaurate in (5) is 1:1.3-2.2:0.2-0.3; The weight ratio of the intermediate product A, methyl benzoyl chloride and the catalyst triethanolamine in (6) is 1:2.3-2.5:0.3-0.6; The fluorine source in (7) is one or more of sodium fluoride, ammonium fluoride, and potassium fluoride; the phosphorus source is one or more of ammonium phosphate, potassium dihydrogen phosphate, and sodium dihydrogen phosphate; the vanadium source is vanadium trioxide, vanadium oxalate, and ammonium vanadate; and the lithium source is one or more of lithium acetate, lithium oxalate, lithium carbonate, and lithium hydroxide.