A preparation method of electrocatalytic cathode material and its application
By preparing electrode materials with foam nickel-loaded precious metal Pd and oxygen-rich vacancies tricobalt tetroxide nanocone, the existing Pd-based electrocatalyst material has been solved, and the efficient electrocatalytic addition of chlorine organic pollutants has been achieved. Hydrochlorination reduces costs and improves catalytic stability.
Patent Information
- Application Number
- CN202311173573.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-12
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-09-12
AI Technical Summary
The existing Pd-based electrocatalyst materials have low yield and poor selectivity for hydrogen atoms (H*), resulting in low electrocatalytic hydrochloride dechlorination efficiency of chlorinated organic pollutants, and the high cost and low reserves of palladium limit their Large-scale application in water treatment.
Using an electrocatalytic cathode material preparation method, the Co support solution is prepared by dissolving palladium chloride powder with cobalt nitrate hexahydrate, ammonium fluoride and urea in deionized water, and then soaking through hydrothermal reaction, calcination and sodium borohydride. , Co3O4-OV/NF carrier material is formed, and then ultraviolet light irradiated with load Pd to prepare electrode materials with foam nickel-loaded precious metal Pd and oxygen-rich vacancies tricobalt tetoxide nanocone.
Improves the selectivity of H* and electrocatalytic hydrodechlorination performance, with low loading and low cost. The hydrodechlorination efficiency of Pd@Co3O4-OV/NF material for 2,4-dichlorophenol can reach 130 minutes. 95.40%, showing excellent anti-interference ability and catalytic stability.
Smart Images

Figure CN117181241B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrocatalytic hydrogenation dechlorination, and in particular to a preparation method of an electrocatalytic cathode material and application thereof. Background Art
[0002] Chlorinated organic compounds (COCs) are widely used in the fields of pesticides, chemicals, electronics, oil refining, and medicine. However, most organochlorine compounds have the disadvantages of being difficult to degrade, highly bioaccumulative, and highly toxic, which seriously affect the environment and even endanger human health. Electrocatalytic hydrodechlorination (EHDC) treatment has the advantages of high efficiency, mild reaction conditions, low equipment cost, and no secondary pollution. It is considered to be one of the most promising methods for treating chlorinated organic pollutants in water.
[0003] EHDC is an indirect reduction reaction pathway initiated by the in-situ generation of active atomic hydrogen (H*) on the surface of specific cathode materials through the reduction of H+. As a highly reduced species, H* reduces the toxicity of COCs by cleaving the C-Cl bond in COCs. For the electrocatalytic hydrodechlorination of pollutants, most of the reported studies focus on the use of the precious metal Pd, because it has the efficiency and durability to generate H* from aqueous solution in a wide pH range compared to other precious metals, and it exhibits strong adsorption and activation ability for halogenated pollutants in subsequent hydrodechlorination reactions. It is recognized as one of the most effective electrocatalytic hydrodechlorination precious metals. However, studies on the kinetics and electrochemical behavior of H* on Pd nanoparticle catalysts have shown that only a small part of the generated H* can be used for EHDC, and most of them generate hydrogen through the hydrogen evolution side reaction, resulting in low utilization of H*. In addition, the high cost and low reserves of palladium also limit its large-scale practical application in water treatment. Designing a reasonable Pd structure to change the charge environment while improving the yield and selectivity of H* and the atomic utilization of Pd has important research significance and application prospects for effectively treating chlorinated organic pollutants in water to alleviate water pollution. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing an electrocatalytic cathode material and its application, so as to solve the problems of low yield and poor selectivity of Pd-based electrocatalyst materials prepared by the prior art for H* and low atomic utilization of Pd.
[0005] The purpose of the present invention is achieved through the following technical solutions:
[0006] A method for preparing an electrocatalytic cathode material comprises the following steps:
[0007] Cobalt nitrate hexahydrate, ammonium fluoride and urea powder were dissolved in deionized water, and the mixture was stirred thoroughly to obtain a Co carrier solution. The Co carrier solution and a piece of nickel foam (NF) were transferred to a polytetrafluoroethylene high-pressure hydrothermal reactor, and a Co precursor / NF material was hydrothermally prepared in an oven. The Co precursor / NF material was dried and calcined in a tube furnace to obtain a Co3O4 / NF material. The Co3O4 / NF material was immersed in a sodium borohydride solution, and after the reaction was completed, it was repeatedly washed with deionized water and dried to obtain a Co3O4 / NF material. 4-OV / NF carrier material; palladium chloride powder is added into deionized water, and then an appropriate amount of hydrochloric acid is added to stir and dissolve to obtain a Pd precursor solution; Co3O 4-OV The / NF carrier material was placed in a Pd precursor solution, and then loaded with Pd by ultraviolet light to obtain Pd@Co3O 4-OV / NF material.
[0008] Furthermore, when the Co carrier solution is prepared, the amount of cobalt nitrate hexahydrate is 2-4 mmol, the amount of ammonium fluoride is 3-5 mmol, the amount of urea is 7-8 mmol, and the amount of deionized water is 30-50 ml.
[0009] Furthermore, when preparing the Co precursor / NF material, the Co carrier solution is mixed with a 2.25-4 cm 2 , the nickel foam with a thickness of 0.5 to 1 mm is transferred to a polytetrafluoroethylene high-pressure hydrothermal reactor with a volume of 50 to 100 ml, and then hydrothermally heated at a hydrothermal temperature of 130 to 150°C for 4 to 8 hours.
[0010] Furthermore, when preparing Co3O4 / NF material, the temperature is raised from room temperature to 350-400°C at a heating rate of 2-5°C / min in an air atmosphere through a tubular furnace, and then the Co precursor / NF material is calcined at a temperature of 350-400°C for 2-3h.
[0011] Further, the preparation of Co3O 4-OV / NF carrier material, the Co3O4 / NF material is placed in a sodium borohydride solution with a concentration of 0.75-2 mol / L and immersed for 2-4 hours, and then heated at 60°C for 6 hours for drying after washing.
[0012] Furthermore, when preparing the Pd precursor solution, palladium chloride powder is added to deionized water to prepare a Pd solution with a concentration of 0.4 to 0.6 mmol / L, and then hydrochloric acid with a concentration of 0.8 to 1.2 mmol / L is added to the Pd solution and stirred to finally prepare a Pd precursor solution with a volume of 25 to 30 ml.
[0013] Furthermore, Pd@Co3O 4-OV / NF materials, Co3O 4-OV The mixed solution of the NF support material and the Pd precursor solution is irradiated for 1 to 2 hours.
[0014] Furthermore, the electrode material of nickel foam loaded with precious metal Pd and oxygen-vacancy cobalt tetroxide nanocones prepared based on the above preparation method can be used as a catalyst for electrocatalytic hydrogenation dechlorination treatment of chlorinated organic pollutants in water.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] 1. The electrocatalytic cathode material (Pd@Co3O4-OV / NF) prepared by the preparation method of the present invention is a nickel foam surface grown with oxygen-rich vacancy cobalt oxide nanocones loaded with precious metal Pd. By loading a very small amount of precious metal Pd (loading amount of 0.02536 mg cm -2 ), which makes it have high H* selectivity and electrocatalytic hydrodechlorination performance. The hydrodechlorination efficiency of 2,4-dichlorophenol can reach 95.40% within 130min, and it shows excellent anti-interference ability and catalytic stability.
[0017] 2. The preparation process of the present invention is simple, the cost is low, the obtained product has excellent performance and good electrochemical stability, and has broad prospects for promotion and application in the electrocatalytic hydrogenation dechlorination and detoxification of chlorinated organic pollutants in water. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 Pd@Co3O 4-OV / SEM image of NF;
[0019] Figure 2 Pd@Co3O 4-OV / NF high-resolution transmission electron microscopy image;
[0020] Figure 3 Pd@Co3O 4-OV / NF、Pd@Co3O4 / NF、Co3O 4-OV / NF linear scanning curve comparison in 0.05mol / L Na2SO4 solution;
[0021] Figure 4 Pd@Co3O 4-OV / NF linear scanning curve before and after adding chlorinated organic pollutant 2,4-dichlorophenol in 0.05M Na2SO4 solution;
[0022] Figure 5 Pd@Co3O 4-OV / NF、Pd@Co3O4 / NF、Co3O 4-OV / NF Comparison of the removal efficiency test results of the electrocatalytic hydrodechlorination experiment for the chlorinated organic pollutant 2,4-dichlorophenol (80ppm);
[0023] Figure 6 Pd@Co3O 4-OV / NF Removal efficiency test results of electrocatalytic hydrodechlorination experiment for different initial concentrations of 2,4-dichlorophenol (80ppm);
[0024] Figure 7 Pd@Co3O 4-OV / NF Monitoring results of the total amount of substances changed during the electrocatalytic hydrodechlorination experiment for the chlorinated organic pollutant 2,4-dichlorophenol (80ppm);
[0025] Figure 8 Pd@Co3O 4-OV / NF Anti-anion interference electrocatalytic hydrodechlorination test results for chlorinated organic pollutant 2,4-dichlorophenol (80ppm);
[0026] Fig. 9 Pd@Co3O 4-OV / NF Electrocatalytic hydrodechlorination test results of 2,4-dichlorophenol (80ppm) in different initial pH solutions;
[0027] Fig.10 Pd@Co3O 4-OV / NF electrocatalytic hydrodechlorination test results for 80ppm different halogenated pollutants;
[0028] Fig.11 Pd@Co3O 4-OV / NF Stability test results of five consecutive electrocatalytic hydrodechlorination cycles for 2,4-dichlorophenol (80ppm). DETAILED DESCRIPTION
[0029] The present invention is further described below in conjunction with the accompanying drawings, but the protection scope of the present invention is not limited to the following description. Embodiment 1:
[0030] An electrocatalytic cathode material (Pd@Co3O 4-OV / NF) preparation method, comprising the following steps:
[0031] 1. Preparation of Co3O 4-OV / NF carrier material, the specific steps are:
[0032] ① Dissolve cobalt nitrate hexahydrate, ammonium fluoride and urea powder in deionized water, stir thoroughly and prepare a Co carrier solution. The amount of cobalt nitrate hexahydrate is 2-4 mmol, the amount of ammonium fluoride is 3-5 mmol, the amount of urea is 7-8 mmol, and the amount of deionized water is 30-50 ml.
[0033] In this embodiment, the amount of cobalt nitrate hexahydrate used is 2 mmol, the amount of ammonium fluoride used is 3 mmol, the amount of urea used is 7 mmol, and the amount of deionized water used is 30 ml.
[0034] ②. Transfer the Co carrier solution and a piece of nickel foam (NF) to a polytetrafluoroethylene high-pressure hydrothermal reactor, and hydrothermally prepare the Co precursor / NF material in an oven.
[0035] More specifically, when preparing Co precursor / NF material, the Co carrier solution is mixed with a 2.25-4 cm 2 , the nickel foam with a thickness of 0.5 to 1 mm is transferred to a polytetrafluoroethylene high-pressure hydrothermal reactor with a volume of 50 to 100 ml, and then hydrothermally heated at a hydrothermal temperature of 130 to 150°C for 4 to 8 hours.
[0036] In this embodiment, the size of the nickel foam used is 1.5*1.5 cm 2 , thickness is 1mm; the volume of the polytetrafluoroethylene high-pressure hydrothermal reactor is 50ml; the hydrothermal temperature is 130℃, and the hydrothermal time is 4h.
[0037] ③. After drying the Co precursor / NF material, place it in a tube furnace for calcination to obtain Co3O4 / NF material.
[0038] More specifically, when preparing Co3O4 / NF material, the temperature is raised from room temperature to 350-400°C at a heating rate of 2-5°C / min in an air atmosphere through a tubular furnace, and then the Co precursor / NF material is calcined at 350-400°C for 2-3h.
[0039] In this embodiment, the tube furnace was heated from room temperature to 350° C. at a heating rate of 2° C. / min in an air atmosphere, and then the Co precursor / NF material was calcined at 350° C. for 2 h.
[0040] ④. Soak the Co3O4 / NF material in sodium borohydride solution. After the reaction is completed, wash it repeatedly with deionized water and dry it to obtain Co3O4 / NF. 4-OV / NF carrier material.
[0041] More specifically, the preparation of Co3O 4-OV / NF carrier material, the Co3O4 / NF material is placed in a sodium borohydride solution with a concentration of 0.75-2 mol / L and immersed for 2-4 hours, and then heated at 60°C for 6 hours for drying after washing.
[0042] In this embodiment, the concentration of the sodium borohydride solution used is 0.75 mol / L, and the immersion time is 2 h. During the immersion process, NaBH4 is oxidized according to the reaction equation 8M. n+ +NaBH4+2H2O→8M (n-1)+ +NaBO2+8H + Reduce the high-valent metal ions in the metal oxide, thereby generating oxygen vacancies to maintain the overall charge balance of the material.
[0043] 2. Prepare the Pd precursor solution. The specific steps are as follows:
[0044] Add palladium chloride powder into deionized water, then add a proper amount of hydrochloric acid and stir to promote dissolution, so as to obtain a Pd precursor solution.
[0045] More specifically, when preparing the Pd precursor solution, palladium chloride powder is added to deionized water to prepare a Pd solution with a concentration of 0.4 to 0.6 mmol / L, and then hydrochloric acid with a concentration of 0.8 to 1.2 mmol / L is added to the Pd solution for stirring, and finally a Pd precursor solution with a volume of 25 to 30 ml is prepared, wherein the Pd element exists in the solution in the form of PdCl4 which is easily reduced by light. 2- .
[0046] In this embodiment, 25 ml of Pd precursor solution was prepared, wherein the concentration of the Pd solution was 0.4 mmol / L, the concentration of hydrochloric acid was 0.8 mmol / L, and the stirring time was 6 h.
[0047] 3. UV light reduction of loaded Pd, the specific steps are:
[0048] Co3O 4-OV The / NF carrier material was placed in a Pd precursor solution, and then loaded with Pd by ultraviolet light to obtain Pd@Co3O 4-OV / NF material.
[0049] More specifically, the preparation of Pd@Co3O 4-OV / NF materials, Co3O 4-OV The mixed solution of the NF support material and the Pd precursor solution was irradiated for 1 to 2 h, thereby the adsorbed PdCl4 2- The ions are anchored at the oxygen vacancies.
[0050] In this embodiment, the wavelength of the ultraviolet light is 365 nm, the irradiation time is 1 h, and the Pd loading is 0.02536 mg cm-2 UV light reduction is conducive to the formation of stable and dispersed low-noble metal-loaded catalysts, thereby promoting catalytic performance while reducing preparation costs. Compared with the use of chemical reducing agents for reduction, it is safer and more environmentally friendly.
[0051] like Figure 1 As shown, it can be observed through scanning electron microscopy that the electrocatalytic cathode material (Pd@Co3O 4-OV / NF) showed nano-dimensional growth on its surface, and no obvious Pd nanoparticles were observed on the surface, indicating a low loading of Pd.
[0052] like Figure 2 As shown, it can be observed through high-resolution transmission electron microscopy that the electrocatalytic cathode material (Pd@Co3O 4-OV The lattice spacing of Pd was captured in the lattice fringes of the nanostructured Pd / NF (Figure 5A), demonstrating the successful loading of Pd.
[0053] Under the action of metal-support interaction, electron transfer and redistribution can occur between Pd and the support, and electrons are transferred from the support to Pd, thereby improving the generation and adsorption capacity of H* on the electron-rich Pd surface and improving the selectivity of H* for the EHDC process. At the same time, there are a large number of defects and holes on the support surface, which can provide a strong binding position for anchoring the precious metal Pd nanoparticles, which is beneficial to improving the stability and utilization of Pd atoms. In this regard, the present invention can provide sufficient H* for the electrocatalytic hydrogenation and dechlorination of chlorinated organic pollutants by using Co3O4 material rich in oxygen vacancies as a support. The strong metal-support interaction between Co3O4 and Pd can effectively improve the electronic environment of Pd, and the formed electron-rich Pd can effectively improve the selectivity of H*. The oxygen vacancy defects on Co3O4 can stabilize the precious metal atom Pd to reduce the amount of Pd and improve the utilization of Pd. Finally, the electronic environment of the precious metal is adjusted by constructing a strong metal-support interaction, and then the catalytic selectivity of the active center is adjusted, so that the electrocatalytic cathode material (Pd@Co3O 4-OV / NF) can be used as a catalyst with high catalytic performance and applied in the electrocatalytic hydrodechlorination treatment of chlorinated organic pollutants in water.
[0054] The electrocatalytic cathode material (Pd@Co3O 4-OV / NF) was used as the electrochemical cathode, and 2,4-dichlorophenol was selected as the reactant for the electrocatalytic hydrodechlorination experiment. The reaction was carried out in a conventional H-type double-chamber electrolyzer and tested using a multi-channel electrochemical analyzer. Specifically, the anode and cathode chamber cells were separated by a Nafion-117 membrane. The cathode chamber contained 40 mL Na2SO4 (50 mM) and 2,4-dichlorophenol (80 mg L −1) aqueous solution, the anode chamber contains 40mL Na2SO4 (50mM) solution. Platinum sheet (1.5*1.5cm 2 ) and Ag / AgCl electrodes were used as the anode and reference electrodes of the electrolytic cell, respectively. Before the test, the solutions in the cathode and anode chambers were saturated with N2. During the electrolysis, the cathode electrolyte was magnetically stirred at a constant current of 10 mA cm -2 The working time at room temperature is 2 hours. 0.5 mL of sample was taken out from the cathode chamber at regular intervals and analyzed by high performance liquid chromatography at a wavelength of 275 nm. The mobile phase was 70% methanol and 30% water at a flow rate of 1.0 mL min -1 . Embodiment 2:
[0055] Based on the preparation method in Example 1, this embodiment provides a method for preparing an electrode material (Pd@Co3O4 / NF) in which cobalt oxide nanocones are grown on the surface of nickel foam and loaded with precious metal Pd, comprising the following steps:
[0056] 1. Prepare Co3O4 / NF carrier material, the specific steps are:
[0057] ①. Dissolve 2mmol of cobalt nitrate hexahydrate, 3mmol of ammonium fluoride and 7mmol of urea powder in 30ml of deionized water and stir thoroughly to obtain a Co carrier solution.
[0058] ②, mix the Co carrier solution with a piece of 1.5*1.5 cm 2 , nickel foam (NF) with a thickness of 1 mm was transferred to a polytetrafluoroethylene high-pressure hydrothermal reactor with a volume of 50 ml, and then hydrothermally heated in an oven at a hydrothermal temperature of 130°C for 4 h to prepare a Co precursor / NF material.
[0059] ③. After drying the Co precursor / NF material, place it in a tube furnace. The tube furnace is heated from room temperature to 350°C at a heating rate of 2°C / min in an air atmosphere. The Co precursor / NF material is calcined at 350°C for 2h to obtain Co3O4 / NF material.
[0060] 2. Prepare the Pd precursor solution. The specific steps are as follows:
[0061] Add palladium chloride powder into deionized water to prepare a Pd solution with a concentration of 0.4 mmol / L, then add an appropriate amount of hydrochloric acid with a concentration of 0.8 mmol / L into the Pd solution and stir to promote dissolution, so as to prepare 25 ml of a Pd precursor solution.
[0062] 3. UV light reduction of loaded Pd, the specific steps are:
[0063] The Co3O4 / NF carrier material was placed in a Pd precursor solution, and then the mixed solution of the Co3O4 / NF carrier material and the Pd precursor solution was irradiated with ultraviolet light with a wavelength of 365nm for 1h to load Pd, thereby obtaining a Pd@Co3O4 / NF material.
[0064] Based on the experimental and test conditions in Example 1, the electrode material (Pd@Co3O4 / NF) prepared in this example, in which cobalt oxide nanocones were grown on the surface of nickel foam and loaded with precious metal Pd, was used as an electrochemical cathode, and 2,4-dichlorophenol was selected as a reactant for an electrocatalytic hydrogenation dechlorination experiment. The reaction was carried out in a conventional H-type double-chamber electrolyzer and tested using a multi-channel electrochemical analyzer. Embodiment three:
[0065] Based on the preparation method in Example 1, this embodiment provides an electrode material (Co3O4) having oxygen-rich vacancy cobalt oxide nanocones grown on the surface of nickel foam. 4-OV The preparation method of the composite material comprises the following steps:
[0066] ①. Dissolve 2mmol of cobalt nitrate hexahydrate, 3mmol of ammonium fluoride and 7mmol of urea powder in 30ml of deionized water and stir thoroughly to obtain a Co carrier solution.
[0067] ②, mix the Co carrier solution with a piece of 1.5*1.5 cm 2 , nickel foam (NF) with a thickness of 1 mm was transferred to a polytetrafluoroethylene high-pressure hydrothermal reactor with a volume of 50 ml, and then hydrothermally heated in an oven at a hydrothermal temperature of 130°C for 4 h to prepare a Co precursor / NF material.
[0068] ③. After drying the Co precursor / NF material, place it in a tube furnace. The tube furnace is heated from room temperature to 350°C at a heating rate of 2°C / min in an air atmosphere. The Co precursor / NF material is calcined at 350°C for 2h to obtain Co3O4 / NF material.
[0069] ④. Soak the Co3O4 / NF material in a 0.75 mol / L sodium borohydride solution for 2 h to obtain Co3O4 / NF. 4-OV / NF carrier material.
[0070] Based on the experimental and test conditions in Example 1, the electrode material (Co3O4) with oxygen-rich vacancy cobalt tetroxide nanocones grown on the surface of the nickel foam prepared in this example 4-OV / NF) was used as the electrochemical cathode and 2,4-dichlorophenol was selected as the reactant for the electrocatalytic hydrodechlorination experiment. The reaction was carried out in a traditional H-type double-chamber electrolyzer and tested using a multi-channel electrochemical analyzer.
[0071] According to experiments and tests, the above Pd@Co3O 4-OV / NF、Pd@Co3O4 / NF、Co3O 4-OV The linear scanning curves of the three materials / NF in 0.05mol / L Na2SO4 solution are shown in Figure 3 As shown, it can be seen that Pd@Co3O 4-OV The current density of Pd@Co3O4 / NF is higher than that of Co3O4 / NF and Pd@Co3O4 / NF. 4-OV / NF current density, indicating that in Pd@Co3O 4-OV / NF electrode greatly promotes the generation of H*. 4-OV The linear scanning curve of the NF material before and after adding the chlorinated organic pollutant 2,4-dichlorophenol in 0.05M Na2SO4 solution is shown in Figure 2. Figure 4 As shown in the figure, it can be seen that the introduction of 2,4-dichlorophenol leads to an increase in the cathode current density, indicating that Pd@Co3O 4-OV / NF has higher selectivity for the electrocatalytic hydrodechlorination of 2,4-dichlorophenol than for the hydrogen evolution reaction (HER).
[0072] Pd@Co3O 4-OV / NF、Pd@Co3O4 / NF、Co3O 4-OV The removal efficiency test results of the electrocatalytic hydrodechlorination experiment of the three materials / NF for the chlorinated organic pollutant 2,4-dichlorophenol (80ppm) are as follows Figure 5 As shown, it can be seen that compared with Pd@Co3O4 / NF and Co3O 4-OV / NF,Pd@Co3O 4-OV / NF has a higher electrocatalytic hydrodechlorination efficiency for 2,4-dichlorophenol at 130 min, while Pd@Co3O4 / NF has a hydrodechlorination efficiency of 95.40% for 2,4-dichlorophenol at 130 min. 4-OV The removal efficiency test results of the electrocatalytic hydrodechlorination experiment for different initial concentrations of 2,4-dichlorophenol (80ppm) are shown in Figure 6 As shown in the figure, it can be seen that higher concentrations of 2,4-dichlorophenol will limit the 4-OV Electrocatalytic hydrodechlorination performance of / NF.
[0073] Pd@Co3O 4-OV / NF Monitoring results of the total amount of substances (2,4-dichlorophenol, o-chlorophenol and phenol) during the electrocatalytic hydrodechlorination experiment of chlorinated organic pollutants 2,4-dichlorophenol (80ppm) are as follows Figure 7As shown, it can be seen that Pd@Co3O 4-OV / NF For the chlorinated organic pollutant 2,4-dichlorophenol (80ppm) during the electrocatalytic hydrodechlorination experiment, the total concentration of the substance remained basically unchanged, indicating that the electrocatalytic hydrodechlorination had few side reactions.
[0074] Pd@Co3O 4-OV / NF for the chlorinated organic pollutant 2,4-dichlorophenol (80ppm) anti-anion interference electrocatalytic hydrodechlorination test results are as follows Figure 8 As shown, it can be seen that SO3 2- It has a limiting effect on electrocatalytic hydrodechlorination, while other anions have little effect on the reaction.
[0075] Pd@Co3O 4-OV The electrocatalytic hydrodechlorination test results of 2,4-dichlorophenol (80 ppm) in different initial pH solutions are shown in Figure 2. Fig. 9 As shown, it can be seen that Pd@Co3O 4-OV The electrocatalytic hydrodechlorination performance of / NF has good pH adaptability.
[0076] Pd@Co3O 4-OV The electrocatalytic hydrodechlorination test results of NF for 80ppm different halogenated pollutants (4-fluorophenol, 2-bromophenol, 2-chlorophenol and 4-chlorophenol) are as follows Fig.10 As shown, it can be seen that, except for 2-chlorophenol, Pd@Co3O 4-OV / NF has a high hydrodechlorination efficiency for the other three halogenated organic pollutants.
[0077] Pd@Co3O 4-OV / NF stability test results for five consecutive electrocatalytic hydrodechlorination cycles of 2,4-dichlorophenol (80ppm) are shown in Fig.11 As shown, it can be seen that Pd@Co3O 4-OV / NF has good electrocatalytic hydrodechlorination cycle stability.
[0078] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An application of an electrocatalytic cathode material, characterized in that: The electrocatalytic cathode material is used as a catalyst for electrocatalytic hydrodechlorination of chlorinated organic pollutants in water. The preparation method of the electrocatalytic cathode material comprises the following steps: Dissolve 2-4 mmol of cobalt nitrate hexahydrate, 3-5 mmol of ammonium fluoride and 7-8 mmol of urea powder in 30-50 ml of deionized water, and stir thoroughly to prepare a Co carrier solution; The Co carrier solution and a piece of nickel foam NF were transferred to a polytetrafluoroethylene high-pressure hydrothermal reactor, and the Co precursor / NF material was hydrothermally prepared in an oven; The Co precursor / NF material is dried and then calcined in a tube furnace to obtain a Co3O4 / NF material; The Co3O4 / NF material was placed in a sodium borohydride solution with a concentration of 0.75-2 mol / L and soaked for 2-4 hours. After the reaction was completed, it was repeatedly washed with deionized water and dried at 60°C for 6 hours to obtain Co3O4 / NF. 4-OV / NF carrier material; Add palladium chloride powder to deionized water to prepare a Pd solution with a concentration of 0.4 to 0.6 mmol / L, then add hydrochloric acid with a concentration of 0.8 to 1.2 mmol / L to the Pd solution and stir, and finally prepare a Pd precursor solution with a volume of 25 to 30 ml; Co3O 4-OV The / NF carrier material was placed in a Pd precursor solution, and then loaded with Pd by ultraviolet light to obtain Pd@Co3O 4-OV / NF material.
2. The use of the electrocatalytic cathode material according to claim 1, characterized in that: When preparing Co precursor / NF material, the Co carrier solution is mixed with a 2.25-4 cm 2 , the nickel foam with a thickness of 0.5 to 1 mm is transferred to a polytetrafluoroethylene high-pressure hydrothermal reactor with a volume of 50 to 100 ml, and then hydrothermally heated at a hydrothermal temperature of 130 to 150° C. for 4 to 8 hours.
3. The use of the electrocatalytic cathode material according to claim 1, characterized in that: When preparing Co3O4 / NF material, the temperature is raised from room temperature to 350-400°C at a heating rate of 2-5°C / min in an air atmosphere through a tubular furnace, and then the Co precursor / NF material is calcined at a temperature of 350-400°C for 2-3h.
4. The use of the electrocatalytic cathode material according to claim 1, characterized in that: Preparation of Pd@Co3O 4-OV / NF materials, Co3O 4-OV The mixed solution of the NF support material and the Pd precursor solution is irradiated for 1 to 2 hours.