Composite adsorption material and preparation method and application thereof
By growing PBAs in situ on porous alumina microspheres to form composite adsorption materials, the problem of difficult application of existing PBAs powders in chromatographic columns is solved, and efficient adsorption and separation of cesium ion is achieved, suitable for removing environmentally friendly environments. Radioactive cesium.
Patent Information
- Application Number
- CN202311098676.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-29
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-08-29
AI Technical Summary
The existing Prussian blue analogues (PBAs) powders are small and difficult to apply in chromatographic columns, resulting in low adsorption and separation efficiency of cesium ions and poor performance in high salt conditions, affecting its effect on removing radioactive cesium in the environment.
PBAs are grown in situ on porous alumina microspheres, and composite adsorption materials are formed by precipitation and hydrothermal treatment. The load volume is controlled between 20 and 30 wt%, to improve adsorption capacity and mechanical stability. It is suitable for adsorption of cesium ions in liquid waste. Separation.
It significantly improves the adsorption capacity and adsorption performance of cesium ions, reduces the pressure drop of the adsorption bed, and achieves efficient cesium ions removal. It has a simple and economical process and is suitable for industrial applications.
Smart Images

Figure BDA0004420112850000051 
Figure HDA0004420112860000011 
Figure HDA0004420112860000012
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of cesium removal, and specifically to a composite adsorption material and a preparation method and application thereof. Background Art
[0002] To meet the growing demand for energy, the nuclear industry has flourished and plays a key role in the world's electricity production. However, nuclear waste and accidents lead to the release of radionuclides ( 137 Cs, 90 Sr. 235 U. 57 The leakage of radionuclides into the environment has always been a serious and thorny problem. 137 Cs has a half-life of 30 years, high-energy β / γ-release (0.514MeV and 0.662MeV), high solubility, and is easy to enter the human body, leading to an increase in the incidence of cancer, leukemia, and other diseases. For example, the Chernobyl accident in 1986 and the Fukushima accident in 2011 137 The leakage and serious discharge of Cs have caused serious impacts on the local environment, and the surrounding area is still listed as a hazardous area. Therefore, removing radioactive substances from wastewater is necessary. 137 Cs is of great significance to human health and environmental protection.
[0003] Prussian blue was first synthesized more than three centuries ago, and many Prussian blue analogs have been discovered and studied over the years. Compared with organic resins or zeolites, PBAs have good adsorption properties for cesium. Even in high salt conditions, they have a high affinity for cesium over a wide pH range and have good resistance to ionizing radiation. Cu-Fe Prussian blue analogs have a high affinity for cesium over a wide pH range due to their lattice size. and cesium ions The size matching allows it to selectively adsorb cesium.
[0004] However, there are some problems in the application of PBAs. PBAs are fine powders and have a large pressure drop in the chromatographic column, making them difficult to apply to actual adsorption separation. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention provides a composite adsorbent material and a preparation method and application thereof. In the present invention, PBAs are grown in situ on porous alumina microspheres, the preparation method is simple and easy, the reaction conditions are mild and the reaction process is controllable, the prepared composite adsorbent material is environmentally friendly, simple in process, economical to use, suitable for chromatographic column adsorption and separation of radioactive cesium in liquid waste, has a high adsorption capacity for cesium ions, has excellent chemical and mechanical stability, and can obtain a higher decontamination coefficient.
[0006] In a first aspect, a composite adsorption material is provided, comprising alumina microspheres and a Prussian blue analogue loaded on the surface and / or inside of the alumina microspheres, wherein the Prussian blue analogue is a ferrocyanide of a transition metal.
[0007] In some embodiments, the Prussian blue analog is one or more of potassium copper ferrocyanide, potassium nickel ferrocyanide, and potassium cobalt ferrocyanide.
[0008] The inventors have found through a large number of experiments that potassium copper ferrocyanide has high industrial application potential while maintaining its performance, and its raw materials copper ferrocyanide and copper nitrate are cheap and easily available. In some embodiments, the Prussian blue analog is potassium copper ferrocyanide.
[0009] In some embodiments, the Prussian blue analog is crystalline.
[0010] In some embodiments, the loading amount of the Prussian blue analogue is 20-30 wt %, for example, 20 wt %, 22 wt %, 24 wt %, 26 wt %, 28 wt %, 30 wt %.
[0011] In some embodiments, the diameter of the alumina microspheres is 1 to 2 mm.
[0012] In a second aspect, a method for preparing a composite adsorbent material is provided, comprising:
[0013] (1) precipitating transition metal elements onto the surface of alumina to obtain transition metal-loaded alumina;
[0014] (2) In situ growth of a Prussian blue analogue on the transition metal-loaded alumina to obtain the composite adsorption material.
[0015] In some embodiments, the method for preparing the transition metal-loaded alumina comprises: mixing alumina with urea and a transition metal salt solution to precipitate the transition metal onto the surface of the alumina to obtain the transition metal-loaded alumina.
[0016] In some embodiments, the method of precipitating a transition metal onto the alumina surface comprises impregnation, deposition precipitation, and hydrothermal treatment.
[0017] In some embodiments, the copper salt is selected from one or more of copper nitrate, copper chloride or copper sulfate.
[0018] In some embodiments, the nickel salt is selected from one or more of nickel nitrate, nickel chloride or nickel sulfate.
[0019] In some embodiments, the cobalt salt is selected from one or more of cobalt nitrate, cobalt chloride or cobalt sulfate.
[0020] In some embodiments, the mass ratio of alumina to urea is (3-10):1; for example, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1.
[0021] In some embodiments, the molar ratio of the aluminum oxide to the transition metal salt is (1-5):1, for example, 1:1, 2:1, 3:1, 4:1, or 5:1.
[0022] In some embodiments, the aluminum oxide is pretreated before use, and the pretreatment step includes: ultrasonically treating the aluminum oxide with hydrochloric acid or sodium hydroxide solution, and then drying.
[0023] Preferably, the concentration of the hydrochloric acid is 1-2M; for example, 1M, 1.2M, 1.4M, 1.6M, 1.8M, 2M.
[0024] Preferably, the ultrasonic treatment time is 30 to 60 min, for example, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min.
[0025] In some embodiments, the temperature for mixing alumina with urea and transition metal salt solution is 65-85°C, for example 65°C, 70°C, 77°C, 80°C, 83°C, 85°C.
[0026] In some embodiments, the in situ growth process comprises:
[0027] S1, mixing the transition metal-loaded alumina, potassium ferrocyanide and a solvent,
[0028] S2, adding transition metal salt solution and potassium ferrocyanide,
[0029] S3, repeat step S2 at least once to obtain the composite adsorption material.
[0030] In some embodiments, in step S1, the temperature of mixing the loaded transition metal, potassium ferrocyanide and solvent is 25°C-60°C, for example, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, and the mixing time is 20 to 48 h, for example, 20 h, 25 h, 30 h, 35 h, 40 h, 45 h, 48 h.
[0031] In some embodiments, the solvent is water.
[0032] In some embodiments, step S2 is repeated 1 to 3 times.
[0033] In some embodiments, the volume ratio of the transition metal salt to the potassium ferrocyanide is (0.5-2):1; for example, 0.5:1, 0.7:1, 0.9:1, 1.1:1, 1.3:1, 1.5:1, 1.7:1, 1.9:1, 2:1.
[0034] In some embodiments, the molar ratio of the transition metal salt to the potassium ferrocyanide is (1-3):1, for example, 1:1, 1.5:1, 2:1, 2.5:1, or 3:1.
[0035] In a third aspect, there is provided a use of the composite adsorption material described in the first aspect or the composite adsorption material prepared by the preparation method described in the second aspect in removing cesium ions.
[0036] The composite adsorption material provided by the present invention uses alumina microspheres as a matrix. Compared with powdered PBAs, the PBAs adsorption material in situ grown on porous alumina has excellent mechanical strength and a honeycomb porous structure, can significantly reduce the bed pressure drop of the adsorption bed, and also has a high adsorption capacity and cycle stability.
[0037] The present invention grows PBAs in situ on porous alumina microspheres, and at the same time, urea is added during the growth of PBAs powder, and the concentrations of urea and metal cations are adjusted to make them grow evenly on the alumina spheres. The preparation method is simple and easy, the reaction conditions are mild, and the reaction process is controllable. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 It is the adsorption test performance diagram of the powdered Cu-Fe PBAs and the Prussian blue analogue@alumina composite adsorption material obtained in Example 1.
[0039] Figure 2 Figure 2 shows untreated alumina microspheres (left) and the Prussian blue analog @ alumina composite adsorbent material obtained in Example 1 (right).
[0040] Figure 3 This is the SEM image of the Prussian blue analogue@alumina composite adsorption material obtained in Example 1.
[0041] Figure 4 This is the Fourier infrared diffraction test pattern of the Prussian blue analogue@alumina composite adsorption material obtained in Example 1. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments and drawings. The specific embodiments described herein are only used to explain the present invention and are not intended to constitute any limitation to the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concepts of the present disclosure. Such structures and technologies are also described in many publications.
[0043] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0044] The present invention will be described in detail below through examples.
[0045] Example 1
[0046] First, 1g of alumina (1-2mm) was soaked in 1mol / L hydrochloric acid solution for 30 minutes and vacuum dried overnight. The treated alumina microspheres, 0.2g Cu(NO3)2·3H2O, 0.2g urea, and 50mL deionized water were added to a 100mL reactor and reacted at 75℃ for 24h to make copper evenly deposited on the surface of alumina. After washing away the excess copper salt with deionized water, vacuum dried for 24h, 0.2g potassium ferrocyanide and 50mL deionized water were added to grow PBAs on the surface of alumina, and reacted at 75℃ for 24h to make the surface of alumina covered with PBAs. Wash again to remove the excess potassium ferrocyanide, vacuum dried, add 50mL solution containing 0.2g copper nitrate and react for 24h; after washing and drying, add potassium ferrocyanide and react for 24h. Repeat the deposition 1-2 times to make PBAs grow on the surface of alumina. The aforementioned microspheres were washed with deionized water and vacuum dried for 24 hours to obtain an alumina-Prussian blue analog composite microsphere adsorption material. Figure 3 As shown, Fourier transform infrared spectroscopy characterizes the functional group structure of the material, such as Figure 4 shown. Figure 4 This indicates that the alumina-Prussian blue analog composite microsphere adsorption material of the present invention has the same structure as the Prussian blue analog. Figure 3 and Figure 4 All of them prove that Prussian blue analogs are supported on alumina.
[0047] The adsorption performance of alumina-Prussian blue analogue composite microsphere adsorption material and Prussian blue analogue is as follows Figure 1As shown, it can be seen that the adsorption performance of the alumina-Prussian blue analog composite microsphere adsorption material prepared by the present invention is significantly improved.
[0048] Alumina-Prussian blue analogue composite microsphere adsorption material and alumina such as Figure 2 shown.
[0049] Example 2
[0050] First, 1g of alumina (1-2mm) was soaked in 1mol / L sodium hydroxide solution for 30 minutes and vacuum dried overnight. The treated alumina microspheres, 0.2g Cu(NO3)2·3H2O, 0.2g urea, and 50mL deionized water were added to a 100mL reactor and reacted at 75℃ for 24h to make copper evenly deposited on the surface of alumina. After washing away the excess copper salt with deionized water, vacuum dried for 24h, 0.2g potassium ferrocyanide and 50mL deionized water were added to grow PBAs on the surface of alumina, and the reaction was continued for 24h to make the surface of alumina covered with PBAs. Wash again to remove the excess potassium ferrocyanide, vacuum dried, add 50mL solution containing 0.2g copper nitrate and react for 24h; after washing and drying, potassium ferrocyanide was added and reacted for 24h. Repeat the deposition 1-2 times to make PBAs grow on the surface of alumina. The aforementioned microspheres were washed with deionized water and vacuum dried for 24 hours to obtain an alumina-Prussian blue analog composite microsphere adsorption material.
[0051] Example 3
[0052] Different from Example 1, the loading amount of the Prussian blue analogue was 30%.
[0053] First, 1g of alumina (1-2mm) was soaked in 1mol / L hydrochloric acid solution for 30 minutes and vacuum dried overnight. The treated alumina microspheres, 0.4g Cu(NO3)2·3H2O, 0.4g urea, and 50mL deionized water were added to a 100mL reactor and reacted at 75℃ for 24h to make copper evenly deposited on the surface of alumina. After washing away the excess copper salt with deionized water, vacuum dried for 24h, 0.2g potassium ferrocyanide and 50mL deionized water were added to grow PBAs on the surface of alumina, and the reaction was continued for 24h to make the surface of alumina covered with PBAs. Wash again to remove the excess potassium ferrocyanide, vacuum dried, add 50mL solution containing 0.2g copper nitrate and react for 24h; after washing and drying, potassium ferrocyanide was added and reacted for 24h. Repeat the deposition 1-2 times to make PBAs grow on the surface of alumina. The aforementioned microspheres were washed with deionized water and vacuum dried for 24 hours to obtain an alumina-Prussian blue analog composite microsphere adsorption material.
[0054] Comparative Example 1
[0055] An untreated Prussian blue analogue was used.
[0056] Adsorption performance test: 0.3 g of PBAs@Al2O3 prepared in the above embodiments was weighed into a cone, added into 10 mL of 25 ppm cesium chloride simulated solution, and shaken at 150 rpm for 24 h, as shown in Table 1.
[0057] Table 1
[0058]
[0059] From the above examples and Table 1, it can be seen that the adsorption capacity of PBAs@Al2O3 prepared by the present invention for cesium ions can reach 60.2 mg / g, which has great industrial application prospects. In the experiment of adsorption separation of 25ppm simulated cesium solution, cesium can be removed by more than 99.2%.
[0060] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A composite adsorption material comprising alumina microspheres and a Prussian blue analogue loaded on the surface and / or inside of the alumina microspheres, wherein the Prussian blue analogue is a ferrocyanide of a transition metal; The Prussian blue analogue is potassium copper ferrocyanide; The Prussian blue analog is a crystal; the loading amount of the Prussian blue analog is 20-30wt%; the particle size of the alumina microspheres is 1-2mm; The preparation method of the composite adsorption material comprises: (1) Precipitating transition metal elements onto the surface of alumina to obtain transition metal-loaded alumina; (2) in situ growing a Prussian blue analog on the transition metal-loaded alumina to obtain the composite adsorption material; The preparation method of the transition metal-loaded aluminum oxide comprises: mixing aluminum oxide with urea and a transition metal salt solution to precipitate the transition metal on the surface of the aluminum oxide to obtain the transition metal-loaded aluminum oxide, wherein the transition metal salt is selected from copper salt; the mass ratio of the aluminum oxide to urea is (3-10):1; the molar ratio of the urea to the transition metal salt is (1-5):1; the temperature of mixing the aluminum oxide with the urea and the transition metal salt solution is 65-85°C; The aluminum oxide is pretreated before use, and the pretreatment step includes: ultrasonically treating the aluminum oxide with hydrochloric acid; the concentration of the hydrochloric acid is 1-2M; The in-situ growth process includes: S1, mixing the transition metal-loaded alumina, potassium ferrocyanide and a solvent, S2, adding transition metal salt solution and potassium ferrocyanide, S3, repeating step S2 at least once to obtain the composite adsorption material; in step S1, the temperature of mixing the transition metal-loaded alumina, potassium ferrocyanide and solvent is 25°C to 60°C, and the mixing time is 20 to 48 hours; The molar ratio of the transition metal salt to the potassium ferrocyanide is (1-3):
1.
2. The composite adsorption material according to claim 1, characterized in that: The copper salt is selected from one or more of copper nitrate, copper chloride or copper sulfate.
3. The composite adsorption material according to claim 1, characterized in that: The ultrasonic treatment time is 30 to 60 minutes.
4. The composite adsorption material according to claim 1, characterized in that: The solvent is water.
5. The composite adsorption material according to claim 1, characterized in that: The number of times step S2 is repeated is 1 to 3 times.
6. Use of the composite adsorbent material according to any one of claims 1 to 5 in removing cesium ions.