A Ce, Ga, Mo co-doped CaBi4Ti4O 15 High temperature piezoelectric ceramic material and preparation method thereof
By co-doping CaBi4Ti4O15 high-temperature piezoelectric ceramic materials in Ce, Ga and Mo, the problem of insufficient Curie temperature and piezoelectric activity of high-temperature piezoelectric ceramic materials in the existing technology is solved, and the improvement of high-temperature stability and comprehensive electrical performance is achieved. Suitable for high temperature environments.
Patent Information
- Application Number
- CN202311186211.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-14
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-09-14
AI Technical Summary
The Curie temperature of the existing perovskite structure PZT-based piezoelectric ceramic materials is generally below 400℃, which cannot work normally in high temperature environments. The piezoelectric activity of bismuth layered ceramic materials is low, which limits its high temperature field. Application.
Using Ce, Ga and Mo co-doped CaBi4Ti4O15 high-temperature piezoelectric ceramic material, the Ca2+ ions are replaced by 12-coordinated high-valent Ce4+ ion doping, and the composite high-valent ion [Ga1/3Mo2/3]5+ doping replaces Ti4+ ions to form Ca1-xCexBi4Ti4-y[Ga1/3Mo2/3]yO15 improves its piezoelectric performance and high temperature resistivity.
While not reducing the Curie temperature, the piezoelectric activity and high-temperature resistivity of piezoelectric ceramic materials are significantly improved. The material's d33≥28pC/N, TC≥775℃, and the resistivity at 500℃ is ≥3.5×107Ω·cm. Dielectric loss is ≤0.35%, suitable for high temperature applications.
Smart Images

Figure CN117263679B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of piezoelectric ceramic materials, and in particular to a bismuth calcium titanate high-temperature piezoelectric ceramic material with a bismuth layered structure and a preparation method thereof. Background Art
[0002] At present, the most widely used piezoelectric ceramic materials are mainly PZT-based piezoelectric ceramics with perovskite structure, but the Curie temperature of this type of piezoelectric ceramics is generally below 400℃. Due to the existence of depolarization phenomenon of piezoelectric materials, piezoelectric materials cannot work normally above the Curie temperature. With the rapid development of aerospace, geological exploration and other work and in line with the needs of sustainable development of human society, it is necessary to seek an environmentally friendly piezoelectric material with high Curie temperature and excellent piezoelectric performance.
[0003] Bismuth layered ceramics have the advantages of high Curie temperature and good fatigue resistance, and are candidate materials for use in high temperature environments. Bismuth layered ceramics are made of (Bi2O2) 2+ The layers and perovskite structure lattice layers are alternately stacked, and its chemical formula is (Bi2O2) 2+ (A m-1 B m O 3m+1 ) 2- , among which, CaBi4Ti4O 15 (CBT) is a typical bismuth layered ferroelectric material, A is a 12-coordinated Ca 2+ and Bi 3+ , B is 6-coordinated Ti 4+ , m = 4, the material has a high Curie temperature (T C ≈790℃), high voltage coefficient, low conductivity and other advantages, but its piezoelectric activity is low and the temperature coefficient of resonance frequency is large, which restricts its application in high temperature fields. Therefore, how to improve the piezoelectric activity without reducing the Curie temperature and obtain CBT piezoelectric ceramic materials with excellent comprehensive electrical properties has become an important research topic in the field of high temperature piezoelectric ceramic materials. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a Ce, Ga, and Mo co-doped CaBi4Ti4O 15 High temperature piezoelectric ceramic materials, for CaBi4Ti4O 15 Ca in the A position of ceramic materials 2+ ions, using high-valent Ce with 12 coordination 4+ Ions are used for doping substitution, targeting Ti at the B site 4+ ions, using composite high-valent ions [Ga 1 / 3 Mo 2 / 3 ]5+ Doping substitution is performed so that through the above-mentioned composite doping modification, the piezoelectric properties and high-temperature resistivity are improved without reducing the Curie temperature, thereby providing a new type of environmentally friendly piezoelectric ceramic material with excellent comprehensive electrical properties. Another object of the present invention is to provide the above-mentioned Ce, Ga, Mo co-doped CaBi4Ti4O 15 Preparation method of high temperature piezoelectric ceramic material.
[0005] The purpose of the present invention is achieved through the following technical solutions:
[0006] The present invention provides a Ce, Ga, Mo co-doped CaBi4Ti4O 15 High temperature piezoelectric ceramic materials, with 12-coordinated high-priced Ce 4+ Ion doping replaces CaBi4Ti4O 15 Ca in the A position 2+ ions, with complex high-valent ions [Ga 1 / 3 Mo 2 / 3 ] 5+ Doped substituted CaBi4Ti4O 15 Ti in the middle B position 4+ ions, the chemical formula is Ca 1-x Ce x Bi4Ti 4-y [Ga 1 / 3 Mo 2 / 3 ] y O 15 , where 0.045≤x≤0.075, 0.05≤y≤0.075.
[0007] In the above scheme, the piezoelectric ceramic material of the present invention has a 33 ≥28pC / N, T C ≥775℃; Resistivity (ρ) ≥3.5×10 at 500℃ 7 Ω@cm, dielectric loss (tanδ) ≤ 0.35%; d after annealing at 600℃ 33 ≥24pC / N.
[0008] Another object of the present invention is achieved by the following technical solutions:
[0009] The Ce, Ga, and Mo co-doped CaBi4Ti4O 15 A method for preparing a high temperature piezoelectric ceramic material comprises the following steps:
[0010] (1) Preparation of pre-synthesized precursor powder
[0011] CaCO3, CeO2, Bi2O3, TiO2, Ga2O3, and MoO3 are used as raw materials corresponding to Ca, Ce, Bi, Ti, Ga, and Mo in the chemical formula, and each raw material is mixed according to the stoichiometric amount in the chemical formula, and then a ball milling treatment is performed using anhydrous ethanol as a ball milling medium, and the obtained material is dried, sieved, pressed and formed, and then placed in a sealed crucible for calcination; then the calcined material is ground and sieved, and a second ball milling treatment is performed, and the obtained material is dried, ground, and sieved to obtain a pre-synthesized precursor powder;
[0012] (2) Preparation of high temperature piezoelectric ceramic materials
[0013] The pre-synthesized precursor powder is loaded into a graphite mold, and placed in a spark plasma sintering furnace for a primary calcination treatment to obtain a carbon-containing sintered product; then the carbon-containing sintered product is placed in an ordinary high-temperature furnace for a secondary calcination treatment to decarbonize, to obtain a decarbonized sintered product; finally, the decarbonized sintered product is polarized to obtain a high-temperature piezoelectric ceramic material.
[0014] Furthermore, the purity of each raw material in step (1) of the preparation method of the present invention is not less than 99.9%. The pressure of the pressing molding is 4-6Mpa; and the calcination treatment is to increase the temperature to 800-850°C at 5°C / min.
[0015] Furthermore, in the step (2) of the preparation method of the present invention, the primary calcination treatment is performed by heating the spark plasma sintering furnace at a pressure of 25 to 30 MPa and a DC pulse current of 500 to 550 A to 800 to 850° C. at 100° C. / min, keeping the temperature for 5 to 8 minutes, stopping the DC pulse current, releasing the pressure, and cooling the furnace to room temperature. The secondary calcination treatment is performed by heating the temperature to 600 to 650° C. at 5° C. / min, keeping the temperature for 3 to 4 hours, and cooling the furnace to room temperature.
[0016] Furthermore, the polarization treatment in step (2) of the preparation method of the present invention is to first polish the surface of the decarbonized sintered product; then perform electrode coating treatment, that is, silver electrodes are applied to the upper and lower surfaces of the decarbonized sintered product after polishing; then calcine at 650-680°C at 5°C / min, keep warm for 40-60min, and cool to room temperature with the furnace; finally, polarize in high-temperature silicone oil at 180-200°C with a DC voltage of 5-10kV / mm for 20-30min.
[0017] Using the Ce, Ga, Mo co-doped CaBi4Ti4O 15 Products obtained by the preparation method of high-temperature piezoelectric ceramic materials.
[0018] The present invention has the following beneficial effects:
[0019] (1) In the preparation of CaBi4Ti4O 15 In the process of preparing piezoelectric ceramic materials, due to the volatilization of bismuth at high temperature, bismuth vacancies will inevitably be formed, thereby generating vacancy defects. In view of this phenomenon, the present invention adopts a valence ratio of A-site Ca 2+ Ce with high ions 4+ Ions are doped and replaced, and the valence ratio of B-site Ti is also used. 4+ Ion high composite ion [Ga 1 / 3 Mo 2 / 3 ] 5+ Doping and substitution are performed to make the A and B positions both defective, making the perovskite layer (A m-1 B m O 3m+1 ) 2- Generates electrons, thereby strengthening the bismuth oxide layer (Bi2O2) 2+ and perovskite-like layers (A m-1 B m O 3m+1 ) 2- The interaction between them changes the growth behavior of the grains, and finally the CaBi4Ti4O with excellent performance is obtained. 15 High temperature piezoelectric ceramic materials.
[0020] (2) The present invention adopts advanced spark plasma sintering technology, which requires low sintering temperature and short sintering time, thus low energy consumption, and high density of the sintered material, and can obtain CaBi4Ti4O with excellent performance. 15 High temperature piezoelectric ceramic materials.
[0021] (3) Ce, Ga, and Mo co-doped CaBi4Ti4O 15 Piezoelectric ceramic material, Curie temperature ≥ 775℃, piezoelectric constant d 33 ≥28pC / N, d after annealing at 600℃ 33 ≥24pC / N; resistivity ≥3.5×10 at 500℃ 7 Ω·cm, dielectric loss ≤0.35%. This material has good high temperature stability and has broad application prospects in high temperature fields.
[0022] (4) The preparation method of the present invention adopts advanced ceramic preparation technology, has low firing temperature, low preparation cost, simple and easy process operation, and easy control of influencing factors. It is suitable for large-scale industrial production and is conducive to promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The present invention will be further described in detail below with reference to the embodiments and accompanying drawings:
[0024] Figure 1Ce, Ga, and Mo co-doped CaBi4Ti4O prepared in the embodiment of the present invention 15 XRD patterns of high temperature piezoelectric ceramics and comparative piezoelectric ceramic materials;
[0025] Figure 2 Ce, Ga, and Mo co-doped CaBi4Ti4O prepared in the embodiment of the present invention 15 The curve of dielectric constant variation with temperature of high temperature piezoelectric ceramics. DETAILED DESCRIPTION
[0026] Embodiment 1:
[0027] This embodiment is a Ce, Ga, and Mo co-doped CaBi4Ti4O 15 The preparation method of high temperature piezoelectric ceramic material comprises the following steps:
[0028] (1) Preparation of pre-synthesized precursor powder
[0029] CaCO3, CeO2, Bi2O3, TiO2, Ga2O3, MoO3 with a purity of 99.9% are used as 0.06 Bi4Ti 3.94 [Ga 1 / 3 Mo 2 / 3 ] 0.06 O 15 The raw materials corresponding to Ca, Ce, Bi, Ti, Ga and Mo are prepared according to the chemical quantities in the general chemical formula, and then anhydrous ethanol is used as the ball milling medium, and the ball: material: anhydrous ethanol = 4: 1: 3 is used for a first ball milling treatment on a planetary ball mill at a speed of 400 r / min for 24 hours. The obtained material is dried, passed through an 80-mesh sieve, pressed and formed at 4 MPa, and then placed in a sealed crucible, and the temperature is increased to 800° C. at 5° C. / min and calcined in an oxidizing atmosphere for 2 hours; the calcined material is ground and passed through an 80-mesh sieve, and a second ball milling treatment is performed using the same process as the first ball milling treatment, and the obtained material is dried, ground and passed through an 80-mesh sieve to obtain a pre-synthesized precursor powder;
[0030] (2) Preparation of high temperature piezoelectric ceramic materials
[0031] (2-1) 0.8 g of the above-mentioned pre-synthesized precursor powder was loaded into a cylindrical graphite mold with a diameter of 20 mm, placed in a spark plasma sintering furnace, set the pressure to 25 MPa, and the DC pulse current to 500 A, and heated to 800 ° C at 100 ° C / min for a calcination treatment. After keeping the temperature for 5 min, the DC pulse current was stopped, and then the pressure was released, and the furnace was cooled to room temperature to obtain a carbon-containing sintered product;
[0032] (2-2) placing the carbon-containing sintered product in a common high-temperature furnace, heating the temperature to 600° C. at 5° C. / min for secondary calcination to decarbonize the product, keeping the temperature for 3 hours, and cooling the product to room temperature to obtain a decarbonized sintered product;
[0033] (2-3) The decarburized sintered product is subjected to the following polarization treatment: first, the surface of the decarburized sintered product is polished; then, electrode coating is performed, i.e., silver electrodes are applied to the upper and lower surfaces of the decarburized sintered product after polishing; then, the temperature is raised to 650°C at 5°C / min, the temperature is kept for 40 minutes, and the product is cooled to room temperature with the furnace; finally, the product is polarized in high-temperature silicone oil at 180°C with a DC voltage of 5 to 10 kV / mm for 20 minutes, thereby obtaining a high-temperature piezoelectric ceramic material.
[0034] Embodiment 2:
[0035] This embodiment is a Ce, Ga, and Mo co-doped CaBi4Ti4O 15 The method for preparing high temperature piezoelectric ceramic material is different from that of the first embodiment in that:
[0036] 1. The general chemical formula of this embodiment is Ca 0.95 Ce 0.05 Bi4Ti 3.945 [Ga 1 / 3 Mo 2 / 3 ] 0.055 O 15 .
[0037] 2. The calcination temperature in step (1) is 820°C; the calcination temperature in step (2-1) is 820°C.
[0038] Embodiment three:
[0039] This embodiment is a Ce, Ga, and Mo co-doped CaBi4Ti4O 15 The method for preparing high temperature piezoelectric ceramic material is different from that of the first embodiment in that:
[0040] 1. The general chemical formula of this embodiment is Ca 0.93 Ce 0.07 Bi4Ti 3.93 [Ga 1 / 3 Mo 2 / 3 ] 0.07 O 15 .
[0041] 2. The calcination temperature in step (1) is 820°C; the calcination temperature in step (2-1) is 820°C.
[0042] Comparative Example:
[0043] Undoped, chemical formula CaBi4Ti4O15 A high temperature piezoelectric ceramic material is used as a comparative example, and its preparation steps are the same as those in Example 1.
[0044] The XRD crystal phase spectra of the piezoelectric ceramic materials of the embodiments of the present invention and the comparative examples are as follows: Figure 1 As shown, from Figure 1 It can be seen that the diffraction peaks of the piezoelectric ceramic materials obtained in the embodiments and comparative examples are completely consistent with the standard spectrum PDF 00-052-1640, indicating that the obtained materials are CaBi4Ti4O 15 Material.
[0045] Ce, Ga, and Mo co-doped CaBi4Ti4O prepared in the embodiment of the present invention 15 The dielectric constant of high temperature piezoelectric ceramics varies with temperature. Figure 2 The performance test results of the piezoelectric ceramic materials of the embodiments of the present invention and the comparative examples are shown in Table 1.
[0046] Table 1 Performance of ceramic materials of the embodiments of the present invention and comparative examples
[0047]
Claims
1. A Ce, Ga, Mo co-doped CaBi 4 Ti 4 O 15 Preparation method of high temperature piezoelectric ceramic material, Features: The chemical formula of the piezoelectric ceramic material is Ca 1-x Ce x Bi 4 Ti 4-y [Ga 1 / 3 Mo 2 / 3 ] y O 15 , where 0.045≤x≤0.075, 0.05≤y≤0.075, with a high-valent Ce with 12 coordination 4+ Ion doping replaces CaBi 4 Ti 4 O 15 Ca in the A position 2+ ions, with complex high-valent ions [Ga 1 / 3 Mo 2 / 3 ] 5+ Doping substitution CaBi 4 Ti 4 O 15 Ti in the middle B position 4+ ions; its preparation method comprises the following steps: (1) Preparation of pre-synthesized precursor powder CaCO 3 、CeO 2 、Bi 2 O 3 、TiO 2 , Ga 2 O 3 、MoO 3 As raw materials corresponding to Ca, Ce, Bi, Ti, Ga, and Mo in the chemical formula, each raw material is prepared according to the stoichiometric amount in the chemical formula, and then a ball milling treatment is performed using anhydrous ethanol as a ball milling medium. The obtained material is dried, sieved, pressed and formed under a pressure of 4 to 6 MPa, and then placed in a sealed crucible, and the temperature is increased to 800 to 850° C. at 5° C. / min for calcination. The calcined material is then ground and sieved, and a secondary ball milling treatment is performed. The obtained material is dried, ground, and sieved to obtain a pre-synthesized precursor powder. (2) Preparation of high temperature piezoelectric ceramic materials The pre-synthesized precursor powder is loaded into a graphite mold, and placed in a spark plasma sintering furnace for a calcination treatment, that is, the spark plasma sintering furnace pressure is 25-30 MPa, the DC pulse current is 500-550 A, the temperature is raised to 800-850°C at 100°C / min, and after keeping warm for 5-8 min, the DC pulse current is stopped, and then the pressure is released, and the furnace is cooled to room temperature to obtain a carbon-containing sintered product; then the carbon-containing sintered product is placed in an ordinary high-temperature furnace for a secondary calcination treatment for decarburization, that is, the temperature is raised to 600-650°C at 5°C / min, and the temperature is kept for 3-4 h, and the furnace is cooled to room temperature to obtain a decarburized sintered product; finally, the decarburized sintered product is polarized to obtain a high-temperature piezoelectric ceramic material; the piezoelectric ceramic material corresponds to the A and B positions are replaced by high-priced doping to form A and B position defects, so that the perovskite layer (A m-1 B m O 3m+1 ) 2- Generate electrons to enhance the bismuth oxide layer (Bi 2 O 2 ) 2+ and perovskite-like layers (A m-1 B m O 3m+1 ) 2- The interaction between them changes the growth behavior of the grains.
2. The Ce, Ga, Mo co-doped CaBi according to claim 1 4 Ti 4 O 15 Preparation method of high temperature piezoelectric ceramic material, Features: The purity of each raw material in step (1) is not less than 99.9%.
3. The Ce, Ga, Mo co-doped CaBi according to claim 1 4 Ti 4 O 15 Preparation method of high temperature piezoelectric ceramic material, Features: The polarization treatment in step (2) is as follows: first, the surface of the decarburized sintered product is polished; then, an electrode coating treatment is performed, i.e., silver electrodes are applied to the upper and lower surfaces of the decarburized sintered product after polishing; then, the temperature is raised to 650-680°C at 5°C / min for calcination, the temperature is kept at that temperature for 40-60 min, and the product is cooled to room temperature with the furnace; finally, the product is polarized in high-temperature silicone oil at 180-200°C with a DC voltage of 5-10 kV / mm for a polarization time of 20-30 min.
4. Using the Ce, Ga, Mo co-doped CaBi as claimed in any one of claims 1 to 3 4 Ti 4 O 15 Products obtained by the preparation method of high temperature piezoelectric ceramic materials, Features: The piezoelectric ceramic material d 33 ≥28 pC / N, T C ≥775℃; Resistivity at 500℃( ρ )≥3.5×10 7 Ω·cm, dielectric loss (tan δ )≤0.35%; after annealing at 600℃ d 33 ≥24 pC / N.