A photothermal dual-curing adhesive for electronic precision devices and a preparation method thereof

By using specific formulas and modified silicon micropowders in the adhesive, the problem of insufficient initial adhesion and insufficient adhesion strength after thermal curing of the photothermal double curing adhesive is solved, and rapid photocuring and high adhesion strength are achieved, which is suitable for modern electronic products. process requirements.

CN117264544BActive Publication Date: 2024-12-03COLLTECH DONGGUAN BONDING TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311394994.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-26
Publication Date
2024-12-03
Estimated Expiration
2043-10-26

AI Technical Summary

Technical Problem

The existing photothermal double curing adhesives have problems such as insufficient initial adhesion, insufficient bonding strength after thermal curing, and inconvenient process construction in electronic components, which is difficult to meet the high requirements of modern electronic products.

Method used

Using an adhesive formulation comprising photothermal dual curing compounds, multifunctional acrylate monomers, reactive diluents, photoinitiators, latent curing agents, thermal curing agents, modified silicon micropowders and vapor phase silica, through specific The chemical structure and process treatment of the process achieves rapid photocuring and high initial viscosity, while improving the bonding strength through thermal curing.

Benefits of technology

It achieves rapid photocuring and high initial viscosity, and significantly improves the bonding strength after thermal curing. It is suitable for the use of precision electronic devices, and has resistance to moisture, hot and cold impact and high precision performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117264544B_ABST
    Figure CN117264544B_ABST
Patent Text Reader

Abstract

This invention relates to a photothermal dual-curing adhesive for precision electronic devices and its preparation method. The photothermal dual-curing adhesive comprises the following raw materials: a photothermal dual-curing compound, a multifunctional acrylate monomer, a reactive diluent, isobornyl (meth)acrylate, a photoinitiator, a latent curing agent, a thermosetting agent, fumed silica, modified silica powder, and a black component. The modified silica powder is obtained by modifying silica powder with an alkenyl silane coupling agent and an epoxy silane coupling agent. The photothermal dual-curing compound has the structural formula shown in formula (I). This invention provides a photothermal dual-curing adhesive that combines rapid photocuring and thermocuring while improving bond strength, exhibiting excellent overall performance and good weather resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of adhesives, and in particular relates to a light-heat dual-curing adhesive for electronic precision devices and a preparation method thereof. Background Art

[0002] Various adhesives are needed in electronic components. The development trend of electronic products is becoming more and more miniaturized and functionally integrated, which puts higher requirements on the adhesives used in precision electronic components. Photothermal dual-curing glue is an adhesive that combines the advantages of photocuring and thermal curing. After a few seconds of UV light irradiation, the adhesive can have a high initial adhesion, and then thermal curing is performed. On the one hand, it can cure the areas that cannot be irradiated by UV, and on the other hand, it can further enhance the bonding strength. At present, the photothermal dual-curing adhesive system based on acrylate UV light curing and epoxy resin thermal curing has received a lot of attention and research and development interest in the field of electronic components.

[0003] At present, the photocuring method generally uses UV monomers based on (meth) acrylates, which have a fast UV light-induced polymerization speed and can produce considerable polymerization in a very short illumination time. However, since the adhesive generally contains inorganic fillers, the activity of the thermal curing reaction will be inhibited, so that the adhesion after thermal curing is still small, especially in the thermal curing process at a lower temperature, and satisfactory bonding strength cannot be achieved.

[0004] CN114381208A discloses a photothermal dual-curing adhesive, which uses a multifunctional photocuring compound and a modified epoxy resin, wherein the multifunctional photocuring monomer contains more than two polymerizable unsaturated bonds, the modified epoxy resin contains a hydroxyl group and an isocyanate group, and the equivalent ratio of OH to NCO is 0.5 to 1.5. The patented photothermal dual-curing adhesive has relatively excellent resistance to moisture and heat and cold and heat shock, but the photocuring speed is slow and the initial adhesion is not high.

[0005] CN114507333A discloses a high-toughness, high-weatherability photothermal dual-curing resin, wherein the photothermal dual-curing resin has the following structure (I):

[0006]

[0007] It has three epoxy groups and one carbon-carbon unsaturated double bond. By introducing epoxy groups and double bonds into the silicone chain segment, the glue is endowed with high weather resistance, high heat resistance, impact resistance, hydrophobicity, and corrosion resistance. It also has no small molecule volatiles and is green and environmentally friendly. However, the initial adhesion of light curing cannot meet the current requirements for the assembly of electronic components.

[0008] CN111205777A discloses a trifunctional resin, the structural formula of which is as follows:

[0009]

[0010] It is obtained by the reaction of polyacrylate glycidyl ether, hydroxy vinyl ether and acrylic acid. It utilizes the reaction of epoxy group and hydroxyl or carboxyl group on polyacrylate glycidyl ether to introduce double bonds with photo-initiated polymerization activity into the side chain of polyacrylate glycidyl ether. It overcomes the defect of poor compatibility between photocurable acrylic resin and heat-curable epoxy resin. However, the patent contains both epoxy group and double bond in the photothermal dual-curing active substance, which is a polymer, making the adhesive of the patent have a high viscosity. It still has the defects of inconvenient construction of dispensing process for precision electronic devices and high defect rate.

[0011] The inventor's previous patent CN202311194066.4 discloses a photothermal dual-curing adhesive for a camera module, wherein the functional compound having photocuring and thermal curing has the following structural formula:

[0012]

[0013] Wherein R has an epoxy group and / or a double bond. This patent solves the shortcoming of the light-heat dual-curing adhesive that the initial adhesion is not strong after rapid light curing, but there is still the problem of insufficient bonding strength after thermal curing. Summary of the invention

[0014] In order to realize the domestic substitution solution, the present invention provides a photothermal dual-curing adhesive that can meet the requirements of the camera module AA process. It has a fast photocuring speed and high initial adhesion, high bonding strength after thermal curing, and can withstand high humidity and heat, hot and cold shock, and drop tests. It is very suitable as an adhesive for precision electronic devices, such as camera module AA process. To achieve the above purpose, the present invention provides the following technical solutions:

[0015] A photothermal dual-curing adhesive for electronic precision devices, comprising the following raw materials in parts by weight: 30-40 parts of a photothermal dual-curing compound, 3-5 parts of a multifunctional acrylate monomer, 10-20 parts of a reactive diluent, 5-10 parts of isobornyl (meth)acrylate, 1-5 parts by weight of a photoinitiator, 5-10 parts of a latent curing agent, 10-20 parts of a thermal curing agent, 1-10 parts of fumed silica, 15-20 parts of modified silicon micropowder, and 0.1-1 part of a black material;

[0016] The photothermal dual-curing compound has a structural formula as shown in the following formula (I):

[0017]

[0018] Wherein R is as described in the following formula (II) or formula (III):

[0019]

[0020] wherein R1 and R2 are independently H or -CH3, * represents a bond connected to S; m is an integer between 10 and 20; the quantitative ratio of formula (II) to formula (III) is 2:4 to 4:2; in the present invention, the quantitative ratio of formula (II) to formula (III) is calculated based on the molar ratio of (meth)acrylic acid and six-arm polyethylene glycol thiol added during preparation;

[0021] The modified silicon micropowder is obtained by modifying silicon micropowder with an alkenyl-containing silane coupling agent and an epoxy-containing silane coupling agent.

[0022] Furthermore, the alkenyl-containing silane coupling agent is selected from at least one of vinyl triethoxysilane, vinyl trimethoxysilane, and vinyl triisopropoxysilane, and the epoxy-containing silane coupling agent is selected from at least one of 3-glycidyloxypropyl trimethoxysilane, 3-(2,3-epoxypropyloxy)propyl triethoxysilane, and 3-(2,3-epoxypropyloxy)propyl methyl dimethoxysilane.

[0023] Furthermore, the modified silicon micropowder is prepared by a preparation method comprising the following steps: silicon micropowder is dispersed in an alcohol solvent, an alkenyl-containing silane coupling agent and an epoxy-containing silane coupling agent are added, and the mixture is reacted under a protective atmosphere and under heating and stirring conditions. Furthermore, the alcohol solvent is at least one of methanol and ethanol, the protective atmosphere is nitrogen, the heating and stirring conditions are 50-70°C, and the reaction is carried out at a stirring speed of 500-1000rpm for 5-10h, and the post-treatment after the reaction is completed is filtering, washing, and drying in sequence. Washing is washing with anhydrous ethanol, and drying is vacuum drying.

[0024] Furthermore, the mass ratio of the modified silicon powder, the alkenyl-containing silane coupling agent, and the epoxy-containing silane coupling agent is 100:5-8:7-12.

[0025] Furthermore, the preparation method of the photothermal dual-curing compound refers to the previous patent CN202311194066.4, and is specifically prepared by a preparation method comprising the following steps:

[0026] Six-arm polyethylene glycol thiol and glycidyl (meth)acrylate react under the conditions of photoinitiator and ultraviolet light irradiation; then (meth)acrylic acid is added and reacted in the presence of a catalyst and an inhibitor to obtain a photothermal dual-curing compound; the molar ratio of six-arm polyethylene glycol thiol, glycidyl (meth)acrylate, and (meth)acrylic acid is 1:6.1-6.5:2-4, preferably 1:6.2-6.3:3. More preferably, the number average molecular weight of the six-arm polyethylene glycol thiol is 2000-3000 g / mol.

[0027] The present invention prepares the compound shown in formula (I) containing both epoxy and alkenyl groups, firstly, the thiol (-SH) on the six-arm polyethylene glycol thiol and the alkenyl group of (meth) glycidyl acrylate are used to efficiently prepare an intermediate with an epoxy terminal group through a click chemistry reaction, and then the epoxy terminal group of the intermediate reacts with the carboxyl group of (meth) acrylic acid in the presence of a catalyst and an inhibitor, so that the epoxy terminal groups are converted into alkenyl groups. In this way, a light-heat dual-curing compound containing both epoxy and alkenyl groups is obtained.

[0028] Furthermore, the photoinitiator is DMAP, and the added amount is 1-2wt% of the mass of six-arm polyethylene glycol thiol; the reaction of six-arm polyethylene glycol thiol and glycidyl (meth)acrylate is carried out in an organic solvent, and the reaction conditions are room temperature UV irradiation reaction for 0.5-1h, and the organic solvent is selected from at least one of ethyl acetate and ethylene glycol dimethyl ether; the catalyst is 3,5-diisopropyl chromium salicylate, and the catalyst amount is 0.5-1wt% of the mass of (meth)acrylic acid; the inhibitor is 2,6- Di-tert-butyl-p-methylphenol, the amount of the inhibitor is 3-5wt% of the mass of (meth)acrylic acid; further, the catalyst and the inhibitor are dispersed in the (meth)acrylic acid, and the (meth)acrylic acid containing the catalyst and the inhibitor is slowly added, and the addition is completed in 1-2 hours. The reaction conditions after the addition are to control the temperature at 50-60°C and react for 6-10 hours. When the acid value of the system is less than 5mgKOH / g, the reaction is considered to be completed, and the reaction is cooled and the solvent and unreacted substances are removed by rotary evaporation to obtain a photothermal dual-curing compound shown in formula (I).

[0029] The reactive diluent is selected from at least one of hydroxyl-containing acrylates and epoxy-containing acrylates; preferably, it is a mixture of hydroxyl-containing acrylates and epoxy-containing acrylates in a mass ratio of 1:1-2; more preferably, the epoxy-containing acrylate is selected from at least one of glycidyl methacrylate and 3,4-epoxycyclohexyl methacrylate; the hydroxyl-containing acrylate is selected from at least one of hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate.

[0030] The multifunctional acrylate monomer is at least one selected from 1,6-hexanediol diacrylate, trimethylolpropane triacrylate, and pentaerythritol triacrylate.

[0031] The photoinitiator is selected from at least one of 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexyl benzophenone, 2-methyl-1-(4-methylmercaptophenyl)-2-morpholine-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinephenyl)-1-butanone, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, α,α'-dimethylbenzil ketal, isopropylthioxanthone, benzophenone, methyl o-benzoylbenzoate, and 2,4,6-trimethylbenzoyldiphenylphosphine oxide.

[0032] The thermal curing agent is a thiol curing agent, specifically at least one selected from tetrakis(3-mercaptopropionate)pentaerythritol ester, trimethylolpropane tris(3-mercaptopropionate), 1,4-di(3-mercaptobutyric acid)butane and 1,3,5-tris(3-mercaptobutyric acid)isocyanurate, and polythiol.

[0033] The latent curing agent is selected from one or more of Amicure PN-23, Amicure PN-40, Amicure PN-50, Amicure PN-H produced by Ajinomoto Fine Technology Co., Ltd., Fuji FXE-1000, FXR-1081, FXR-1020, FXR-1030 produced by Fuji Chemical, and EH3293S, EH-5011S, EH4360S, EH-5057PK of ADEKA.

[0034] The fumed silica, as a thixotropic agent, has a specific surface area of ​​100-220 m 2 / g, such as Cabot TS720, Evonik's R202, R972, and Wacker's H20.

[0035] The present invention also provides a method for preparing the photothermal dual-curing adhesive for electronic precision devices, comprising the following steps: putting a photothermal dual-curing compound, a multifunctional acrylate monomer, a reactive diluent, (methyl) acrylate isobornyl, a photoinitiator, a latent curing agent, a thermal curing agent, modified silicon micropowder, and a black material into a double planetary stirring kettle, adding fumed silica after vacuum stirring evenly, and stirring evenly again to obtain the photothermal dual-curing adhesive.

[0036] The excellent effects of the present invention are:

[0037] 1. The light-heat dual-curing adhesive of the present invention is a single component, which avoids the need for on-site preparation of components A and B when using a two-component adhesive; and the adhesive of the present invention has good fluidity and is suitable for the precision dispensing process of electronic components.

[0038] Second, the light-heat dual-curing compound prepared by the present invention contains both epoxy groups and carbon-carbon unsaturated double bonds, and can be cured by light and heat. Rapid light curing also has high initial adhesion, which can meet the process speed of modern industrial production of electronic components, and will not lead to a bottleneck in production process efficiency due to long light curing time.

[0039] 3. After light curing, the active ingredients are further heated for heat curing. The present invention modifies the filler silicon micropowder with epoxy silane and alkenyl silane coupling agent. It has the effects of rapid light curing and heat curing and improves the bonding strength. The obtained adhesive has good comprehensive performance and good weather resistance. It can resist moisture and heat, high and low temperature cycles, and maintain high-precision electronic components from damage. The light-heat dual-curing compound is linked by a flexible polyethylene glycol segment, so that it has a higher cross-linking density after curing and also has better toughness, and has a beneficial anti-drop ability. DETAILED DESCRIPTION

[0040] To make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention will be described in detail below. The following examples are convenient for better understanding of the present invention, but are not intended to limit the present invention. The experimental methods in the following examples are conventional methods unless otherwise specified.

[0041] Unless otherwise specified, the “parts” in the embodiments of the present invention are parts by mass, and the “%” are percentages by mass.

[0042] Preparation Example 1

[0043] 1 mole part of six-arm polyethylene glycol thiol (number average molecular weight 2000) and 6.2 mole parts of glycidyl methacrylate are added into ethylene glycol dimethyl ether, and a photoinitiator DMAP is added (the amount added is 1wt% of the six-arm polyethylene glycol thiol), and the reaction is carried out under 270nm ultraviolet light irradiation for 2h; then 3 mole parts of acrylic acid (containing 3,5-diisopropyl chromium salicylate with 1wt% of the mass of acrylic acid and 2,6-di-tert-butyl-p-methylphenol with 3wt% of the mass of acrylic acid) are slowly added, and the addition is completed within 1h. The temperature is controlled at 60°C for reaction for 6h, and the acid value of the system is less than 5mgKOH / g. The reaction is terminated, cooled, and rotary evaporated to obtain a photothermal dual-curing compound.

[0044] Preparation Example 2

[0045] Other conditions and operations were the same as those in Preparation Example 1, except that the amount of acrylic acid used was 4 parts by mole. The amounts of 3,5-diisopropylchromium salicylate and 2,6-di-tert-butyl-p-methylphenol were recalculated based on the amount of acrylic acid used.

[0046] Preparation Example 3

[0047] Other conditions and operations were the same as those in Preparation Example 1, except that the amount of acrylic acid used was 2 parts by mole. The amounts of 3,5-diisopropyl chromium salicylate and 2,6-di-tert-butyl-p-methylphenol were recalculated according to the amount of acrylic acid used.

[0048] Preparation Example 4

[0049] 100 parts by mass of silicon micropowder (particle size of 5 μm) were dispersed in ethanol, 5 parts by mass of vinyltriethoxysilane and 12 parts by mass of 3-glycidyloxypropyltrimethoxysilane were added, and the mixture was reacted for 7 hours at 50°C and 600 rpm under a nitrogen atmosphere. After the reaction, the mixture was cooled, filtered, washed with ethanol, and vacuum dried to obtain modified silicon micropowder.

[0050] Preparation Example 5

[0051] 100 parts by mass of silicon micropowder (particle size of 5 μm) were dispersed in ethanol, 10 parts by mass of vinyltriethoxysilane and 7 parts by mass of 3-glycidyloxypropyltrimethoxysilane were added, and the mixture was reacted for 7 hours at 50°C and 600 rpm under nitrogen atmosphere. After the reaction, the mixture was cooled, filtered, washed with ethanol, and vacuum dried to obtain modified silicon micropowder.

[0052] Preparation Example 6

[0053] 100 parts by mass of silicon micropowder (particle size of 5 μm) were dispersed in ethanol, and 7 parts by mass of vinyltriethoxysilane and 10 parts by mass of 3-glycidyloxypropyltrimethoxysilane were added. The mixture was reacted for 7 hours at 50°C and 600 rpm under nitrogen atmosphere. After the reaction, the mixture was cooled, filtered, washed with ethanol, and vacuum dried to obtain modified silicon micropowder.

[0054] Comparative Preparation Example 1

[0055] 100 parts by mass of silicon micropowder (particle size of 5 μm) were dispersed in ethanol, 17 parts by mass of vinyltriethoxysilane were added, and the mixture was reacted for 7 hours at 50°C and 600 rpm under a nitrogen atmosphere. After the reaction, the mixture was cooled, filtered, washed with ethanol, and vacuum dried to obtain modified silicon micropowder.

[0056] Comparative Preparation Example 2

[0057] 100 parts by mass of silicon micropowder (particle size of 5 μm) were dispersed in ethanol, 17 parts by mass of 3-glycidyloxypropyltrimethoxysilane were added, and the mixture was reacted for 7 hours at 50°C and 600 rpm under nitrogen atmosphere. After the reaction, the mixture was cooled, filtered, washed with ethanol, and vacuum dried to obtain modified silicon micropowder.

[0058] Example 1

[0059] 40 parts by mass of the photothermal dual-curing compound prepared in Preparation Example 1, 5 parts by mass of pentaerythritol triacrylate, 15 parts by mass of active diluent (the sum of 10 parts by mass of glycidyl methacrylate and 5 parts by mass of hydroxyethyl (meth)acrylate), 8 parts by mass of isobornyl acrylate, 3 parts by mass of 2-hydroxy 2-methyl-1-phenylpropanone, 7 parts by mass of latent curing agent Amicure PN-40, 15 parts by mass of pentaerythritol tetrakis(3-mercaptopropionic acid), 20 parts by mass of modified silica powder prepared in Preparation Example 4, and 0.3 parts by mass of carbon black were added to a double planetary stirring kettle, stirred evenly under vacuum conditions, and then 5 parts by mass of Cabot TS720 were added, stirred evenly again, and sealed and packaged to obtain a photothermal dual-curing adhesive.

[0060] Example 2

[0061] 30 parts by mass of the photothermal dual-curing compound prepared in Preparation Example 1, 5 parts by mass of trimethylolpropane triacrylate, 15 parts by mass of reactive diluent (the sum of 7.5 parts by mass of 3,4-epoxycyclohexyl methacrylate and 7.5 parts by mass of hydroxyethyl (meth)acrylate), 5 parts by mass of isobornyl acrylate, 3 parts by mass of 2-hydroxy 2-methyl-1-phenylpropanone, 5 parts by mass of latent curing agent Amicure PN-23, 10 parts by mass of pentaerythritol tetrakis(3-mercaptopropionic acid), 15 parts by mass of modified silica powder prepared in Preparation Example 4, and 0.3 parts by mass of carbon black were added to a double planetary stirring kettle, stirred evenly under vacuum, and then 5 parts by mass of Wacker H20 were added, stirred evenly again, and sealed and packaged to obtain a photothermal dual-curing adhesive.

[0062] Example 3

[0063] Other conditions and operations are the same as those in Example 1, except that the photothermal dual-curing compound prepared in Preparation Example 1 is replaced by an equal mass of the photothermal dual-curing compound prepared in Preparation Example 2.

[0064] Example 4

[0065] Other conditions and operations are the same as those in Example 1, except that the photothermal dual-curing compound prepared in Preparation Example 1 is replaced by the photothermal dual-curing compound prepared in Preparation Example 3 of equal mass.

[0066] Example 5

[0067] Other conditions and operations are the same as those in Example 1, except that the modified silicon micropowder prepared in Preparation Example 4 is replaced by the modified silicon micropowder prepared in Preparation Example 5 of equal mass.

[0068] Example 6

[0069] Other conditions and operations are the same as those in Example 1, except that the modified silicon micropowder prepared in Preparation Example 4 is replaced by the modified silicon micropowder prepared in Preparation Example 6 of equal mass.

[0070] Example 7

[0071] Other conditions and operations are the same as those in Example 6, except that all 15 parts by mass of the active diluent are glycidyl methacrylate.

[0072] Example 8

[0073] Other conditions and operations are the same as those in Example 6, except that all 15 parts by mass of the active diluent are hydroxyethyl (meth)acrylate.

[0074] Comparative Example 1

[0075] Other conditions and operations are the same as those in Example 6, except that the modified silicon micropowder prepared in Preparation Example 4 is replaced by an equal mass of modified silicon micropowder prepared in Comparative Preparation Example 1.

[0076] Comparative Example 2

[0077] Other conditions and operations are the same as those in Example 6, except that the modified silicon micropowder prepared in Preparation Example 4 is replaced by an equal mass of modified silicon micropowder prepared in Comparative Preparation Example 2.

[0078] Comparative Example 3

[0079] Other conditions and operations are the same as those in Example 6, except that the modified silicon micropowder prepared in Preparation Example 4 is replaced by unmodified silicon micropowder of the same mass.

[0080] Effect example

[0081] The following performance tests were performed on the light-heat dual-curing adhesives obtained in the above examples and comparative examples. The results are shown in Table 1.

[0082] Light curing conditions: 1500mW, 365nm light source, irradiation time 2 seconds;

[0083] Thermal curing conditions: 85℃ for 1h;

[0084] Adhesion test: Adhesion material: 3mm×3mm PC / LCP, thrust machine test;

[0085] Thermal shock test: -40℃ / 1h, 80℃ / 1h, a total of 100 thermal cycles.

[0086] Moisture and heat resistance test: Place under double 85 test conditions (85℃, 85RH%) for 500h.

[0087] After the specimens are light-cured, the bonding strength tested is the initial bonding strength; the bonding strength after heat curing is the final bonding strength. After that, the specimens after light curing and heat curing are subjected to hot and cold shock tests and double 85 humidity and heat tests respectively, and the bonding strength is retested. The loss rate of the final bonding strength is calculated to evaluate the aging resistance of the adhesive.

[0088] Table 1 Performance test of light and heat dual curing adhesive

[0089]

[0090]

[0091] It can be seen that the light-heat dual-curing adhesive provided by the present invention has excellent comprehensive performance, with both rapid light curing and high initial adhesion, and the heat-curing bonding strength is significantly improved by modifying the filler silicon micropowder. It is suitable for use as adhesives for various precision electronic components.

Claims

1. A light-heat dual-curing adhesive for electronic precision devices, characterized in that: The invention comprises the following raw materials in parts by weight: 30-40 parts of a light-heat dual-curing compound, 3-5 parts of a multifunctional acrylate monomer, 10-20 parts of a reactive diluent, 5-10 parts of (meth) acrylate isobornyl, 1-5 parts by weight of a photoinitiator, 5-10 parts of a latent curing agent, 10-20 parts of a thermal curing agent, 1-10 parts of fumed silica, 15-20 parts of modified silicon powder, and 0.1-1 part of a black material; the reactive diluent is selected from at least one of an acrylate containing a hydroxyl group and an acrylate containing an epoxy group; and the black material is carbon black; The photothermal dual-curing compound has a structural formula as shown in the following formula (I): Formula (I) Wherein R is as described in the following formula (II) or formula (III): Formula (II) Formula (III) wherein R1 and R2 are independently H or -CH3, * represents a bond connected to S; m is an integer between 10 and 20; the ratio of the number of formula (II) to formula (III) is 2:4 to 4:2; The modified silicon micropowder is obtained by modifying silicon micropowder with an alkenyl-containing silane coupling agent and an epoxy-containing silane coupling agent.

2. The light-heat dual-curing adhesive for electronic precision devices according to claim 1, characterized in that: The alkenyl-containing silane coupling agent is selected from at least one of vinyl triethoxysilane, vinyl trimethoxysilane and vinyl triisopropoxysilane; The epoxy-containing silane coupling agent is selected from at least one of 3-glycidyloxypropyltrimethoxysilane, 3-(2,3-epoxypropyloxy)propyltriethoxysilane and 3-(2,3-epoxypropyloxy)propylmethyldimethoxysilane.

3. The light-heat dual-curing adhesive for electronic precision devices according to claim 1, characterized in that: The modified silicon micropowder is prepared by a preparation method comprising the following steps: dispersing silicon micropowder in an alcohol solvent, adding an alkenyl-containing silane coupling agent and an epoxy-containing silane coupling agent, and reacting under a protective atmosphere and under heating and stirring conditions.

4. The light-heat dual-curing adhesive for electronic precision devices according to claim 3, characterized in that: The alcohol solvent is at least one of methanol and ethanol, the protective atmosphere is nitrogen, the heating and stirring conditions are 50-70° C., and the reaction is carried out at a stirring speed of 500-1000 rpm for 5-10 hours. After the reaction is completed, the post-treatment is filtering, washing, and drying in sequence, the washing is washing with anhydrous ethanol, and the drying is vacuum drying.

5. The light-heat dual-curing adhesive for electronic precision devices according to claim 1, characterized in that: The mass ratio of the modified silicon micropowder, the alkenyl-containing silane coupling agent, and the epoxy-containing silane coupling agent is 100:5-8:7-12.

6. The light-heat dual-curing adhesive for electronic precision devices according to claim 1, characterized in that: The preparation method of the photothermal dual-curing compound comprises the following steps: Six-arm polyethylene glycol thiol and (meth) glycidyl acrylate react under the conditions of a photoinitiator and ultraviolet light irradiation; then (meth) acrylic acid is added and reacted in the presence of a catalyst and an inhibitor to obtain a photothermal dual-curing compound; the molar ratio of six-arm polyethylene glycol thiol, (meth) glycidyl acrylate, and (meth) acrylic acid is 1:6.1-6.5:2-4.

7. The light-heat dual-curing adhesive for electronic precision devices according to claim 6, characterized in that: The molar ratio of six-arm polyethylene glycol thiol, glycidyl (meth)acrylate and (meth)acrylic acid is 1:6.2-6.3:

3.

8. The light-heat dual-curing adhesive for electronic precision devices according to claim 6, characterized in that: The number average molecular weight of six-arm polyethylene glycol thiol is 2000-3000 g / mol.

9. The light-heat dual-curing adhesive for electronic precision devices according to claim 6, characterized in that: The photoinitiator is DMAP, and the added amount is 1-2wt% of the mass of six-arm polyethylene glycol thiol; the reaction of six-arm polyethylene glycol thiol and glycidyl (meth)acrylate is carried out in an organic solvent, and the reaction conditions are room temperature UV irradiation reaction for 0.5-1h, and the organic solvent is selected from at least one of ethyl acetate and ethylene glycol dimethyl ether; the catalyst is 3,5-diisopropyl chromium salicylate, and the catalyst amount is 0.5-1wt% of the mass of (meth)acrylic acid; the inhibitor is 2,6-di-tert-butyl-p-methylphenol, and the inhibitor amount is 3-5wt% of the mass of (meth)acrylic acid.

10. The light-heat dual-curing adhesive for electronic precision devices according to claim 9, characterized in that: The catalyst and the polymerization inhibitor are dispersed in (meth)acrylic acid, and the (meth)acrylic acid containing the catalyst and the polymerization inhibitor is slowly added and the addition is completed within 1-2 hours. The reaction conditions after the addition are to control the temperature at 50-60°C and react for 6-10 hours. When the acid value of the system is less than 5 mgKOH / g, the reaction is considered to be completed, and the reaction is cooled and the solvent and unreacted substances are removed by rotary evaporation to obtain the photothermal dual-curing compound.

11. The light-heat dual-curing adhesive for electronic precision devices according to claim 1, characterized in that: The active diluent is a mixture of acrylate containing hydroxyl group and acrylate containing epoxy group in a mass ratio of 1:1-2.

12. The light-heat dual-curing adhesive for electronic precision devices according to claim 11, characterized in that: The epoxy-containing acrylate is selected from at least one of glycidyl methacrylate and 3,4-epoxycyclohexyl methacrylate; the hydroxyl-containing acrylate is selected from at least one of hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate and hydroxybutyl (meth)acrylate.

13. The light-heat dual-curing adhesive for electronic precision devices according to claim 1, characterized in that: The multifunctional acrylate monomer is selected from at least one of 1,6-hexanediol diacrylate, trimethylolpropane triacrylate and pentaerythritol triacrylate; The photoinitiator is selected from at least one of 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexyl benzophenone, 2-methyl-1-(4-methylmercaptophenyl)-2-morpholine-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinephenyl)-1-butanone, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, α,α'-dimethylbenzil ketal, isopropylthioxanthone, benzophenone, methyl o-benzoylbenzoate, and 2,4,6-trimethylbenzoyldiphenylphosphine oxide; The thermal curing agent is a thiol curing agent, specifically at least one selected from tetrakis(3-mercaptopropionic acid) pentaerythritol ester, trimethylolpropane tris(3-mercaptopropionate), 1,4-di(3-mercaptobutyric acid) butane and 1,3,5-tris(3-mercaptobutyric acid) isocyanurate, and polythiol; The latent curing agent is selected from one or more of Amicure PN-23, Amicure PN-40, Amicure PN-50, Amicure PN-H produced by Ajinomoto Fine Technology Co., Ltd., Fuji FXE-1000, FXR-1081, FXR-1020, FXR-1030 produced by Fuji Chemical, and EH3293S, EH-5011S, EH4360S, EH-5057PK of ADEKA; The fumed silica, as a thixotropic agent, has a specific surface area of ​​100-220 m 2 / g.

14. The light-heat dual-curing adhesive for electronic precision devices according to claim 13, characterized in that: The fumed silica is selected from Cabot TS720, Evonik's R202, R972 or Wacker's H20.

15. The method for preparing the light-heat dual curing adhesive for electronic precision devices according to any one of claims 1 to 14, characterized in that: The following steps are involved: The photothermal dual-curing compound, multifunctional acrylate monomer, reactive diluent, (meth) acrylate isobornyl, photoinitiator, latent curing agent, thermal curing agent, modified silica powder and black material are put into a double planetary stirring kettle, after vacuum stirring evenly, fumed silica is added, and stirring evenly again to obtain a photothermal dual-curing adhesive.