A Cr 3 C 2 / 25NiCr wear-resistant coating and preparation method thereof

By using explosive spraying technology on the thermal casing of the control rod driving mechanism of the nuclear power reactor, the problem of poor performance of traditional coatings is solved, the preparation of high-performance coatings is achieved, and the use is significantly improved. Lifespan and wear resistance.

CN117265456BActive Publication Date: 2024-11-01超滑科技(佛山)有限责任公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311292943.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-08
Publication Date
2024-11-01
Estimated Expiration
2043-10-08

AI Technical Summary

Technical Problem

The existing wear-resistant coatings prepared through traditional thermal spraying technology have high porosity and low bond strength, which cannot meet the high-performance needs of nuclear power, aerospace and aviation industries.

Method used

Using explosive spraying technology, Cr3C2/25NiCr wear-resistant coating is prepared on the surface of the substrate, hydrogen is used as powder feeding gas, combined with propane and oxygen for explosive spraying, and the oxygen-fuel ratio is controlled between 2.0-2.5 to ensure the sufficient melting of the sprayed material and Vaporize to improve the adhesion and uniformity of the coating.

Benefits of technology

A Cr3C2/25NiCr wear-resistant coating with high hardness and good density is prepared, with low porosity and high bonding strength, which significantly improves the wear resistance and service life of the coating, and is suitable for the surface of complex parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117265456B_ABST
    Figure CN117265456B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of nuclear engineering equipment, and mainly to a Cr3C2 / 25NiCr wear-resistant coating and a preparation method thereof. The preparation method of the Cr3C2 / 25NiCr wear-resistant coating comprises the following steps: using explosion spraying to prepare the Cr3C2 / 25NiCr wear-resistant coating on the surface of the substrate; the fuel gas in the explosion spraying is propane, the combustion-supporting gas is oxygen, and the powder-feeding gas is hydrogen. The preparation method of the Cr3C2 / 25NiCr wear-resistant coating provided in the present application is process-controllable, and can prepare coatings on the surface of large-sized and complex parts, and has important application prospects in the wear resistance of the surface of parts. The coating prepared by the preparation method of the present application has better density and hardness and high bonding strength, which greatly promotes the application of functional coatings in the fields of aerospace and nuclear industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of nuclear engineering equipment, and mainly to a Cr3C2 / 25NiCr wear-resistant coating and a preparation method thereof. Background Art

[0002] The thermowell is a component of the reactor control rod drive mechanism. It is installed above the tube seat of the drive mechanism and has a radial clearance with the tube seat. It is in axial contact with the tube seat without any constraints. When the unit is operating, flow-induced vibration will cause abnormal wear between the thermowell and the tube seat support structure. The wear will extend to the junction of the conical concave surface at the upper end of the tube seat and the upper flange of the thermowell, causing the height position of the thermal insulation sleeve to drop until the upper flange is completely worn away. At that time, the entire thermowell will fall and the remaining annular flange will become a foreign body. In severe cases, a rod jamming accident will occur, that is, the control rods in the reactor cannot be moved up and down to adjust their position.

[0003] In the nuclear power industry, the current solution for this problem in nuclear power plants is generally to directly dismantle the old ones and replace them with new control rod drive wires. However, the replacement of new thermowells takes a long time, the replaced drive wires are highly radioactive, and the replaced drive wires need to be stored and handled separately. The wear and failure of thermowells can be alleviated by preparing wear-resistant coatings at the friction points of thermowells. However, the wear-resistant coatings prepared using traditional thermal spraying technology have high porosity and low bonding strength, and the overall performance of the coating is poor. The prepared wear-resistant coatings cannot meet the needs of large-scale use in industries such as aerospace and aviation, nuclear industry, and supercritical petrochemical equipment.

[0004] Therefore, the prior art still needs to be improved and developed. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the purpose of the present application is to provide a Cr3C2 / 25NiCr wear-resistant coating and a preparation method thereof, aiming to solve the problem of high porosity and low bonding degree of the existing functional coating prepared by traditional thermal spraying technology.

[0006] The technical solution of this application is as follows:

[0007] The present application provides a method for preparing a Cr3C2 / 25NiCr wear-resistant coating, which comprises the following steps:

[0008] The Cr3C2 / 25NiCr wear-resistant coating is prepared on the surface of the substrate by explosion spraying;

[0009] In the explosion spraying, the fuel gas is propane, the combustion-supporting gas is oxygen, and the powder-feeding gas is hydrogen.

[0010] In the present application, hydrogen is used as a powder feeding gas. After the spray material is fed into the combustion chamber, part of the hydrogen is mixed with propane gas to react with oxygen and explode, which is beneficial to provide a high-energy heat source, making the melting and vaporization of the spray material more complete, prompting the spray material to melt rapidly and ensuring the flattening and spreading ability of the spray material droplets, which can improve the adhesion and uniformity of the wear-resistant coating after cooling and solidification, thereby obtaining a high-hardness and dense Cr3C2 / 25NiCr wear-resistant coating.

[0011] Furthermore, the flow rate of the powder feeding gas is 20-40 L / min. The flow rate of the powder feeding gas is 20-40 L / min, which can ensure that the spraying material is effectively fed into the combustion chamber for melting.

[0012] Furthermore, the flow rate of the fuel gas is 20-40L / min; the flow rate of the combustion-supporting gas is 40-50L / min. In the present application, the actual oxygen-fuel ratio at the explosion center can be controlled between 2.0-2.5 by adjusting the flow rates of the fuel gas and the combustion-supporting gas. Under this oxygen-fuel ratio, the propane is not completely burned. The reducing property of hydrogen can ensure that the explosion spraying is carried out in a nearly pure reducing atmosphere, which can prevent the carbide spraying material from decarburization, decomposition or oxidation, reduce the generation of impurities, maintain the original properties of the spraying material, reduce the adverse effects on the wear resistance of the coating, and make the explosion flame in the spraying process more uniform, thereby obtaining a more uniform and dense coating structure and improving the quality of the coating.

[0013] Furthermore, the spraying distance in the explosion spraying is 250-350 mm, the spraying angle is 90°, and the spraying speed is 4-5 mm / s.

[0014] Furthermore, the material of the spray gun outlet section in the explosion spraying is silicon nitride, which is conducive to the rapid escape of the generated water vapor, reduces the impact on the spray material droplets, and ensures that the coating formed by the spraying has a good morphology.

[0015] Furthermore, the substrate is one of Z2CN19-10 nitrogen-controlled austenitic stainless steel or Inconel 718 alloy.

[0016] Furthermore, the substrate is pretreated before the explosion spraying, and the substrate pretreatment is one or more of sandblasting, chemical cleaning and mechanical grinding; the sandblasting material is alumina sand, and the particle size of the alumina sand is 100µm; the chemical cleaning is carried out under ultrasound, and the chemical cleaning reagent is acetone.

[0017] Furthermore, the Cr3C2 / 25NiCr wear-resistant coating is post-processed after preparation, and the post-processing is one of grinding, machining or polishing; after the post-processing is completed, it is also inspected, and the inspection is one or more of visual inspection, thickness gauge inspection and surface roughness meter inspection.

[0018] The present application also provides a Cr3C2 / 25NiCr wear-resistant coating prepared by the preparation method of the Cr3C2 / 25NiCr wear-resistant coating as described above, wherein the thickness of the Cr3C2 / 25NiCr wear-resistant coating is 250-350µm, the Vickers hardness is 600-1000HV, and the fracture toughness is 4-8 MPa×m 1 / 2 , porosity ≤5%.

[0019] Furthermore, the surface roughness Ra of the Cr3C2 / 25NiCr wear-resistant coating ranges from 0.8 to 3.2 µm.

[0020] Beneficial effects: The present application adopts hydrogen as powder feeding gas. The density of hydrogen is relatively low, and a large amount of coating powder for explosion spraying can be transported at a relatively low pressure. In addition, hydrogen has a relatively high thermal conductivity, which is conducive to faster heat conduction during the explosion spraying process, improving the spraying efficiency and reducing energy consumption. At the same time, hydrogen can produce a reducing atmosphere, which is conducive to reducing the oxidation of the coating. The spraying material is not prone to decarburization and decomposition, and the property changes of the hard phase in the coating are reduced, which can ensure the wear resistance of the coating. Hydrogen also has a relatively high combustion rate and can generate a large amount of heat in a relatively short period of time. After the spraying material is fed into the combustion chamber as a powder feeding gas, part of the hydrogen participates in the explosion spraying process as a fuel gas, which is conducive to rapid heating of the powder during the spraying process, and can improve the adhesion and uniformity of the coating. The prepared Cr3C2 / 25NiCr wear-resistant coating has a relatively high density and hardness.

[0021] The preparation method of the Cr3C2 / 25NiCr wear-resistant coating provided in the present application is process-controllable and can be used to prepare surface coatings for large-sized and complex parts. It has important application prospects in the wear resistance of the surface of parts. The Cr3C2 / 25NiCr wear-resistant coating with good comprehensive performance prepared on the thermal sleeve of the control board drive mechanism of a nuclear power reactor by this method can effectively avoid the safety problems of thermal sleeve wear and even failure caused by flow-induced vibration, and the service life is increased by an average of 3-5 times. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a typical indentation photo of the Cr3C2 / 25NiCr wear-resistant coating prepared in this application.

[0023] Figure 2 Schematic diagram of the indentation parameters used to calculate the fracture toughness of the coating.

[0024] Figure 3 This is a cross-sectional scanning electron microscope image of the Cr3C2 / 25NiCr wear-resistant coating prepared in Example 1 of the present application.

[0025] Figure 4 This is a cross-sectional scanning electron microscope image of the Cr3C2 / 25NiCr wear-resistant coating prepared in Example 2 of the present application.

[0026] Figure 5 This is a cross-sectional scanning electron microscope image of the Cr3C2 / 25NiCr wear-resistant coating prepared in Example 3 of the present application. DETAILED DESCRIPTION

[0027] The present application provides a Cr3C2 / 25NiCr wear-resistant coating and a preparation method thereof. To make the purpose, technical solution and effect of the present application clearer and more specific, the present application is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0028] The present application provides a method for preparing a Cr3C2 / 25NiCr wear-resistant coating, which comprises the following steps:

[0029] The Cr3C2 / 25NiCr wear-resistant coating is prepared on the surface of the substrate by explosion spraying;

[0030] The fuel gas in explosion spraying is propane, the combustion-supporting gas is oxygen, and the powder-feeding gas is hydrogen.

[0031] The present application adopts the process of explosion spraying to spray and prepare the Cr3C2 / 25NiCr wear-resistant coating. Compared with plasma spraying and supersonic spraying technology, the explosion spraying material is sprayed at an extremely high speed, and the preparation can be completed in a shorter time, and the production efficiency is higher; due to the extremely high spraying speed, the coating has a very high kinetic energy when it is sprayed onto the surface of the substrate, so that the adhesion between the wear-resistant coating and the substrate is enhanced, and the bonding strength is higher, which is beneficial to improving the durability and protective performance of the coating; explosion spraying can be carried out at a relatively low temperature, which is beneficial to prevent the substrate from being deformed or damaged due to high temperature, and reduce the influence of thermal stress on the wear-resistant coating.

[0032] The coating raw material is Cr3C2 / 25NiCr alloy powder. Cr3C2 / 25NiCr means that the chemical composition of the alloy powder is 75%Cr3C2-25%NiCr, wherein Cr3C2 as a hard phase can provide high wear resistance; NiCr as a bonding phase can provide good coating toughness and corrosion resistance. The Cr3C2 / 25NiCr wear-resistant coating prepared by using Cr3C2 / 25NiCr alloy powder in this ratio has relatively balanced performance, good wear resistance and corrosion resistance, etc., which can meet most coating application requirements and improve the service life of the workpiece.

[0033] The Cr3C2 / 25NiCr wear-resistant coating of the present application can be applied to nuclear energy engineering, so the performance of the Cr3C2 / 25NiCr wear-resistant coating is required to be as good as possible. In view of the above problems, in the present application, the fuel gas in the explosion spraying is propane, the combustion-supporting gas is oxygen, and the powder delivery gas is hydrogen. The present application uses hydrogen as the powder delivery gas, and hydrogen has a wider explosion limit, so that propane with higher convenience, safety and better cost-effectiveness can be selected as the fuel gas, and the combustion temperature of propane is lower than that of acetylene under the explosion condition, and the explosion flame temperature is uniform, avoiding overheating to cause the carbide spray material to decarbonize or cause adverse effects on the substrate. Hydrogen also has a high calorific value. After the spray material is sent into the combustion chamber, part of the hydrogen is also mixed with the propane gas to react with oxygen to explode, which is conducive to providing a high-energy heat source, making the melting and vaporization of the spray material more sufficient and improving the flight speed and impact strength of the molten droplet. Hydrogen also has high thermal conductivity, which means that heat can be transferred to the spraying material more quickly, prompting the spraying material to melt quickly and ensuring the flattening and spreading ability of the spraying material droplets. After cooling and solidification, it can improve the adhesion and uniformity of the wear-resistant coating, thereby obtaining a high-hardness and dense Cr3C2 / 25NiCr wear-resistant coating. It can also reduce energy consumption and effectively improve the spraying efficiency of explosion spraying and the quality of the wear-resistant coating.

[0034] The Cr3C2 / 25NiCr wear-resistant coating is difficult to provide adequate protection when its thickness is low. The thickness of the wear-resistant coating is not only related to the spraying speed and explosion frequency, but also to the powder feeding gas flow rate. When the powder feeding gas flow rate is much lower than the combustion-supporting gas and fuel gas flow rates, due to the setting of the explosion spraying barrel structure, back pressure will be formed in the barrel, making it difficult for the spraying material to be sprayed out, resulting in the thickness of the prepared wear-resistant coating being too low.

[0035] In the present application, the normal powder delivery can be ensured by setting the flow rate of the powder delivery gas to 20-40L / min. The density of hydrogen is relatively low. During the spraying process, hydrogen can be supplied and powdered through the spray gun at a higher flux and speed at a lower pressure. Hydrogen is also partially involved in the explosion spraying process, which helps to increase the spraying speed of the coating, reduce the time of coating formation, improve production efficiency and reduce energy consumption. In addition, with the higher thermal conductivity of hydrogen, hydrogen is kept within the gas flow range to help control the temperature distribution of the coating during the spraying process, reduce the risk of thermal stress in the coating, and help improve the adhesion and durability of the coating.

[0036] Poor control of the oxygen-fuel ratio in conventional explosion spraying will result in the entire spraying process being in an oxidizing atmosphere, resulting in oxidation of the spraying material or substrate, which will change the composition of the spraying material and even affect the properties of the Cr3C2 / 25NiCr wear-resistant coating in this application. In addition, an excessively high oxygen-fuel ratio will also cause Cr3C2 to decompose into chromium-rich products, such as Cr7C3, Cr 23 C6, etc., which in turn affects the hardness and corrosion resistance of the coating. When the oxygen content is low, the fuel gas will not burn completely, the heat released will be reduced, and the powder particles of the sprayed material will not be completely melted. The flying speed of the sprayed material is not fast enough, resulting in poor flattening of the wear-resistant coating. This is manifested in the formation of a non-dense organizational structure on the coating, which ultimately affects the coating's hardness, high-temperature wear resistance and other properties.

[0037] The oxygen-fuel ratio is the main factor affecting the performance of Cr3C2 / 25NiCr wear-resistant coating. Inert gas or compressed air as powder delivery gas will dilute the concentration of the fuel gas and oxygen mixture to a certain extent and reduce the actual oxygen-fuel ratio in explosion spraying after entering the combustion chamber, which will reduce the explosion combustion energy and affect the coating quality. The wear-resistant coating is prone to poor flattening and affects the morphological structure of the coating.

[0038] To address this problem, in this application, the flow rate of fuel gas is 20-40L / min; the flow rate of combustion-supporting gas is 40-50L / min. Explosion spraying equipment, barrel parameters and spraying distance can all affect the oxygen-fuel ratio of explosion spraying. According to the combustion equation in explosion spraying and the structural setting of the spray barrel, explosion combustion is mainly carried out by propane and oxygen in the combustion chamber. The oxygen consumption of hydrogen is not high, but the combustion of the same volume of hydrogen can generate three times the heat of propane, which can provide sufficient energy for explosion spraying, ensure the flight speed of the spray material droplets and the impact strength on the substrate surface. The flight speed of the spray material droplets can be as high as 800~1200m / s, which is beneficial to improve the density and hardness of the Cr3C2 / 25NiCr wear-resistant coating. In the present application, the actual oxygen-fuel ratio at the explosion center can be controlled between 2.0-2.5 by adjusting the flow rates of the fuel gas and the combustion-supporting gas. At this oxygen-fuel ratio, the propane is not completely burned. The reducing property of hydrogen can ensure that the explosion spraying is carried out in a nearly pure reducing atmosphere, which can prevent the carbide spraying material from decarburizing, decomposing or oxidizing, reduce the generation of impurities, maintain the original properties of the spraying material, reduce the adverse effects on the wear resistance of the coating, and make the explosion flame during the spraying process more uniform, thereby obtaining a more uniform and dense coating structure and improving the quality of the coating.

[0039] The propane selected in this application is highly safe and not prone to flashback, and the spraying process of explosion spraying is carried out in a pulsed manner. The explosion spraying equipment used has a good ventilation system. After the pulsed explosion spraying preparation is completed, clean nitrogen will be sent into the combustion chamber for cleaning before the next round of cycle preparation. Therefore, this application uses hydrogen as the powder delivery gas, which has little effect on the overall flashback risk of explosion spraying.

[0040] Furthermore, the spraying distance in explosion spraying is 250-350mm, the spraying angle is 90°, and the spraying speed is 4-5mm / s. Hydrogen with lower density has a higher transmission speed, and the calorific value of explosion spraying with fuel gas is higher, and the spraying efficiency is also higher. Correspondingly, the overall gas flow rate is also relatively high. To match the overall gas flow rate, by adjusting the spraying distance to 250-350mm, the spraying angle to 90°, and the spraying speed to 4-5mm / s, the excessive scattering or sputtering of the spraying material droplets can be reduced, and the utilization rate and spraying efficiency of the spraying material powder can be improved, thereby improving the uniform distribution and coverage of the coating, making it more effectively deposited on the target surface, reducing the gaps and defects in the coating, and being conducive to the good morphological distribution and surface morphology of the coating, forming a dense and non-stratified high-quality wear-resistant coating.

[0041] Furthermore, the material of the spray gun outlet section in explosion spraying is silicon nitride. Propane reacts with oxygen in explosion spraying to generate water, and since the Cr3C2 / 25NiCr spray material is insensitive to water, it will not affect the composition of the wear-resistant coating. However, considering that the powder delivery gas with added hydrogen will produce additional water during the spraying process, if the overall spraying process produces too much water vapor, it may cause changes in the melting and cooling process of the spray material powder, and may also form tiny pores or cracks in the coating, affecting the performance and porosity of the coating. To address this problem, the material of the spray gun outlet section can be set to a high-temperature resistant and dry silicon nitride porous ceramic material, which is conducive to the rapid escape of the generated water vapor, reduces the impact on the molten droplets of the spray material, and ensures that the coating formed by spraying has a good morphology.

[0042] Furthermore, the material of the substrate is one of Z2CN19-10 nitrogen-controlled austenitic stainless steel or Inconel 718 alloy. Inconel 718 is generally added with niobium, and has good corrosion resistance and ductility like Z2CN19-10 nitrogen-controlled austenitic stainless steel, and has stronger bonding with high-speed particles after explosion spraying. High bonding strength is conducive to improving the density and hardness of the Cr3C2 / 25NiCr wear-resistant coating.

[0043] Furthermore, the substrate is pretreated before explosion spraying, and the substrate pretreatment is one or more of sandblasting, chemical cleaning and mechanical grinding. Before explosion spraying, the surface of the substrate is cleaned and any contaminants (such as oil, grease, rust or scale, etc.) are removed, and the substrate surface is treated by processes such as sandblasting, chemical cleaning and mechanical grinding to ensure good adhesion of the substrate surface. Preferably, the sandblasting material is alumina sand, the particle size of the alumina sand is 100µm, the pressure of the compressed air for sandblasting is 0.4~0.6MPa, and the sandblasting distance is controlled between 150-300mm. The surface of the substrate is roughened by sandblasting to further ensure good adhesion of the Cr3C2 / 25NiCr wear-resistant coating to the substrate.

[0044] Furthermore, chemical cleaning is to use acetone to ultrasonically clean the surface of the substrate to remove oil stains, and the pretreated substrate is obtained after drying, and the cleaning is more thorough under ultrasonic conditions.

[0045] Furthermore, the Cr3C2 / 25NiCr wear-resistant coating is also post-processed after preparation. The post-processing can be performed by grinding, machining or polishing to fine-process the coating surface to meet the size requirements of actual use. The surface finish, flatness and surface roughness of the Cr3C2 / 25NiCr wear-resistant coating can also be improved by fine-processing the coating surface. By improving the surface performance of the wear-resistant coating, the use requirements can be further met. Further, grinding is grinding and finishing the Cr3C2 / 25NiCr wear-resistant coating by diamond or boron nitride grinding wheel. Furthermore, before fine processing, impurities on the surface of the substrate are removed by sandblasting, shot peening or high-pressure water cleaning, which can improve the surface flatness and finish of the Cr3C2 / 25NiCr wear-resistant coating and increase the service life of the coating.

[0046] Furthermore, after the post-processing is completed, it is also inspected. The inspection can be carried out by visual inspection, thickness gauge, surface roughness meter and other detection equipment and adhesion test. After cleaning and grinding and polishing, the coating needs to be inspected to ensure that the coating thickness, adhesion, surface roughness and other indicators meet the requirements. The coating thickness is measured by a thickness gauge, the coating Vickers hardness is measured by an HV digital microhardness tester, and the fracture toughness is calculated according to the following formula:

[0047] (Kc / Ha 1 / 2 )(H / E) 1 / 2 =0.028 (C R / a) -3 / 2

[0048] In the formula, Kc represents the fracture toughness, H represents the coating hardness, and E represents the Young's modulus. Figure 1 As shown in the figure, a hardness tester is used to press an indentation on the coating surface. The indentation is rhombus-shaped, and radial cracks grow and extend from the apex of the indentation. Figure 2 As shown, C R It represents the length from the center of the indentation to the top of the indentation, and a represents the straight-line distance from the center of the indentation to the farthest end of the radial crack. C is measured under a magnifying glass. R and a, the fracture toughness can be calculated from the data.

[0049] The preparation method of the Cr3C2 / 25NiCr wear-resistant coating provided by the present application adopts hydrogen as the powder feeding gas. The density of hydrogen is relatively low, and a large amount of coating powder for explosion spraying can be transported at a relatively low pressure. In addition, hydrogen has a relatively high thermal conductivity, which is conducive to faster heat conduction during the explosion spraying process, improving the spraying efficiency and reducing energy consumption. At the same time, hydrogen can produce a reducing atmosphere, and the spraying material is not prone to decarburization and decomposition, which is conducive to reducing the oxidation of the coating. Hydrogen also has a relatively high combustion rate, and can generate a large amount of heat in a relatively short time. After the spraying material is fed into the combustion chamber, part of the hydrogen participates in the explosion combustion as a fuel gas, which is conducive to rapid heating of the powder during the explosion spraying process, and can improve the adhesion and uniformity of the coating. The present application can prepare a coating on the surface of large-sized and complex parts. The prepared Cr3C2 / 25NiCr wear-resistant coating has good comprehensive performance, and also has relatively high density and hardness, and has important application prospects in the wear resistance of the surface of parts.

[0050] The present application also provides a Cr3C2 / 25NiCr wear-resistant coating prepared by the preparation method of the Cr3C2 / 25NiCr wear-resistant coating as described above, wherein the thickness of the prepared Cr3C2 / 25NiCr wear-resistant coating is 250-350µm, the Vickers hardness is 600-1000HV, and the fracture toughness is 4-8 MPa×m 1 / 2 , porosity ≤5%.

[0051] Furthermore, the surface roughness of the post-treated Cr3C2 / 25NiCr wear-resistant coating is within the range of Ra 0.8-3.2µm, which can maintain good surface properties of the Cr3C2 / 25NiCr wear-resistant coating and further extend the service life of the Cr3C2 / 25NiCr wear-resistant coating.

[0052] The Cr3C2 / 25NiCr wear-resistant coating provided in the present application has low porosity and high bonding strength with the substrate. The wear-resistant coating also has the characteristics of high hardness and good comprehensive performance, and has important application prospects in the wear resistance of component surfaces.

[0053] The Cr3C2 / 25NiCr wear-resistant coating described above in this application can also be used in the control rod drive line of a nuclear reactor. In a nuclear reactor, the thermal sleeve of the control rod drive line is affected by the vibration caused by the flow of the loop medium, resulting in intermittent friction between the upper end flange and the CRDM tube seat, so the coating properties are required to be high. This application can prepare a Cr3C2 / 25NiCr wear-resistant coating at the contact point between the thermal sleeve flange and the CRDM tube seat of the control rod drive line. The Cr3C2 / 25NiCr wear-resistant coating has excellent hardness and wear resistance, as well as good toughness. The coating will not crack and fall off and can effectively protect the thermal sleeve flange and the CRDM tube seat, avoiding the safety problem of thermal sleeve wear and even failure caused by flow-induced vibration, and ultimately improving the safety of the reactor and reducing the risk of rod ejection.

[0054] The present application is further described below through specific embodiments.

[0055] Performance testing: Visual inspection, thickness gauge, surface roughness tester and other testing equipment can be used for inspection. The thickness of the Cr3C2 / 25NiCr wear-resistant coating must be within the range of 250-350µm, the Vickers hardness (HV) of the coating must meet the requirements of 600-1000, and the fracture toughness (MPa×m 1 / 2 ) must meet the requirements of 4-8, and the porosity must meet the requirement of ≤5%.

[0056] The thickness of the prepared Cr3C2 / 25NiCr wear-resistant coating was measured by a thickness gauge, the Vickers hardness of the Cr3C2 / 25NiCr wear-resistant coating was measured by an HV digital microhardness tester, and the fracture toughness was calculated according to the following formula: (Kc / Ha 1 / 2 )(H / E) 1 / 2 =0.028 (C R / a) -3 / 2 , Kc represents fracture toughness, H represents coating hardness, E represents Young's modulus, and a hardness tester is used to press an indentation on the coating surface. The indentation is rhombus-shaped, and radial cracks will grow and extend from the top of the indentation. C R It represents the length from the center of the indentation to the top of the indentation, and a represents the straight-line distance from the center of the indentation to the farthest end of the radial crack. C is measured under a magnifying glass. R and a, the fracture toughness can be calculated from the data.

[0057] Example 1

[0058] Surface pretreatment: The workpiece substrate is made of Z2CN19-10 nitrogen-controlled austenitic stainless steel, and the sample sizes are: Ф24mm×8mm and Ф6.35mm×25.4mm. Before spraying, the surface of the workpiece substrate is roughened by sandblasting to ensure good adhesion. The pressure of compressed air is 0.5MPa, the particle size of the aluminum oxide sand used is 100µm, and the sandblasting distance is controlled at 200mm. The surface of the substrate is ultrasonically cleaned with acetone to remove oil stains, and then dried to obtain the pretreated substrate.

[0059] Preparation of coating: Before each explosion, a certain proportion of oxygen and propane combustible mixed gas is first sent into the ignition chamber of the spray gun through the air delivery port, and then the coating powder is sent into the combustion chamber by the powder delivery gas hydrogen through the powder delivery port, and then the combustible mixed gas is ignited by the spark plug to quickly burn and explode, and its heat energy heats the sprayed coating powder to a molten or molten state, and the powder particles at the spray gun mouth are sprayed at a very high speed onto the surface of the workpiece substrate to form a Cr3C2 / 25NiCr wear-resistant coating. After the preparation is completed, clean nitrogen is sent into the combustion chamber for cleaning to prepare for the next preparation work so as to repeat the cycle. The specific process parameters of the explosion spraying of Example 1 are shown in Table 1:

[0060] Table 1

[0061] Explosion frequency (times / s) 6 Spraying distance (mm) 250 Spraying Angle 90° <![CDATA[Fuel gas C3H8 (L / min) (L / MIN)]]> 20 Oxygen (L / min) 42 <![CDATA[Powder feeding gas (H2) (L / min)]]> 20 Spraying speed (mm / s) 4 Coating thickness (µm) 340

[0062] Post-processing: After explosion spraying, the Cr3C2 / 25NiCr wear-resistant coating is ground and finished by diamond or cubic boron nitride grinding wheel to obtain the required size and improve the surface finish and flatness of the Cr3C2 / 25NiCr wear-resistant coating.

[0063] Inspection: After cleaning and grinding and polishing, the Cr3C2 / 25NiCr wear-resistant coating of Example 1 is inspected and its adhesion is tested by visual inspection, thickness gauge, surface roughness gauge and other inspection equipment to ensure that the coating thickness, adhesion, surface roughness and other indicators meet the requirements.

[0064] The performance parameters of the Cr3C2 / 25NiCr wear-resistant coating prepared in Example 1 are shown in Table 2:

[0065] Table 2

[0066] coating Powder Trademark Coating thickness (µm) Coating hardness (HV0.3) <![CDATA[Fracture toughness (MPa×m 1 / 2 )]]> Porosity (%) <![CDATA[Cr3C2 / 25NiCr]]> CDS5260 Lot 210192 320 816 6.7 3 Example 2

[0067] Surface pretreatment: The workpiece substrate is made of Z2CN19-10 nitrogen-controlled austenitic stainless steel, and the sample sizes are: Ф24mm×8mm and Ф6.35mm×25.4mm. Before spraying, the surface of the workpiece substrate is roughened by sandblasting to ensure good adhesion. The pressure of compressed air is 0.5MPa, the particle size of the aluminum oxide sand used is 100µm, and the sandblasting distance is controlled at 200mm. The surface of the substrate is ultrasonically cleaned with acetone to remove oil stains, and then dried to obtain the pretreated substrate.

[0068] Preparation of coating: Before each explosion, a certain proportion of oxygen and propane combustible mixed gas is first sent into the ignition chamber of the spray gun through the air delivery port, and then the coating powder is sent into the combustion chamber through the powder delivery port by the powder delivery gas hydrogen, and then the combustible mixed gas is ignited by the spark plug to quickly burn and explode. The heat energy heats the sprayed coating powder to a molten or molten state, and the powder particles at the spray gun mouth are sprayed at a very high speed onto the surface of the workpiece substrate to form a Cr3C2 / 25NiCr wear-resistant coating. After the preparation is completed, clean nitrogen is sent into the combustion chamber for cleaning to prepare for the next preparation work so as to repeat the cycle. The specific process parameters of the explosion spraying of Example 2 are shown in Table 3:

[0069] Table 3

[0070] Explosion frequency (times / s) 6 Spraying distance (mm) 300 Spraying Angle 90° <![CDATA[Fuel gas C3H8 (L / min) (L / MIN)]]> 20 Oxygen (L / min) 42 <![CDATA[Powder feeding gas (H2) (L / min)]]> 20 Spraying speed (mm / s) 4.5 Coating thickness (µm) 300

[0071] Post-processing: After explosion spraying, the Cr3C2 / 25NiCr wear-resistant coating is ground and finished by diamond or cubic boron nitride grinding wheel to obtain the required size and improve the surface finish and flatness of the Cr3C2 / 25NiCr wear-resistant coating.

[0072] Inspection: After cleaning and grinding and polishing, the Cr3C2 / 25NiCr wear-resistant coating of Example 2 is inspected and its adhesion is tested by visual inspection, thickness gauge, surface roughness meter and other inspection equipment to ensure that the coating thickness, adhesion, surface roughness and other indicators meet the requirements.

[0073] The performance parameters of the Cr3C2 / 25NiCr wear-resistant coating prepared in Example 2 are shown in Table 4:

[0074] Table 4

[0075] coating Powder Trademark Coating thickness (µm) Coating hardness (HV0.3) <![CDATA[Fracture toughness (MPa×m 1 / 2 ).]]> Porosity (%) <![CDATA[Cr3C2 / 25NiCr]]> CDS5260 Lot 210192 300 767 7.3 3 Example 3

[0076] Surface pretreatment: The workpiece substrate is made of Z2CN19-10 nitrogen-controlled austenitic stainless steel, and the sample sizes are: Ф24mm×8mm and Ф6.35mm×25.4mm. Before spraying, the surface of the workpiece substrate is roughened by sandblasting to ensure good adhesion. The pressure of compressed air is 0.5MPa, the particle size of the aluminum oxide sand used is 100µm, and the sandblasting distance is controlled at 200mm. The surface of the substrate is ultrasonically cleaned with acetone to remove oil stains, and then dried to obtain the pretreated substrate.

[0077] Preparation of coating: Before each explosion, a certain proportion of oxygen and propane combustible mixed gas is first sent into the ignition chamber of the spray gun through the air delivery port, and then the coating powder is sent into the combustion chamber through the powder delivery port by the powder delivery gas hydrogen, and then the combustible mixed gas is ignited by the spark plug to quickly burn and explode. The heat energy heats the sprayed coating powder to a molten or molten state, and the powder particles at the spray gun mouth are sprayed at a very high speed onto the surface of the workpiece substrate to form a Cr3C2 / 25NiCr wear-resistant coating. After the preparation is completed, clean nitrogen is sent into the combustion chamber for cleaning to prepare for the next preparation work so as to repeat the cycle. The specific process parameters of the explosion spraying of Example 3 are shown in Table 5:

[0078] Table 5

[0079] Explosion frequency (times / s) 6 Spraying distance (mm) 320 Spraying Angle 90° <![CDATA[Fuel gas C3H8 (L / min) (L / MIN)]]> 20 Oxygen (L / min) 42 <![CDATA[Powder feeding gas (H2) (L / min)]]> 20 Spraying speed (mm / s) 4.8 Coating thickness (µm) 280

[0080] Post-processing: After explosion spraying, the Cr3C2 / 25NiCr wear-resistant coating is ground and finished by diamond or cubic boron nitride grinding wheel to obtain the required size and improve the surface finish and flatness of the Cr3C2 / 25NiCr wear-resistant coating.

[0081] Inspection: After cleaning and grinding and polishing, the Cr3C2 / 25NiCr wear-resistant coating of Example 3 was inspected and its adhesion tested by visual inspection, thickness gauge, surface roughness tester and other inspection equipment to ensure that the coating thickness, adhesion, surface roughness and other indicators meet the requirements.

[0082] The performance parameters of the Cr3C2 / 25NiCr wear-resistant coating prepared in Example 3 are shown in Table 6:

[0083] Table 6

[0084] coating Powder Trademark Coating thickness (µm) Coating hardness (HV0.3) <![CDATA[Fracture toughness (MPa×m 1 / 2 )]]> Porosity (%) <![CDATA[Cr3C2 / 25NiCr]]> CDS5260 Lot 210192 280 885 7.0 4

[0085] The Vickers hardness of the Cr3C2 / 25NiCr coating prepared by explosion spraying in the prior art is generally 500-800HV. Compared with the prior art, the preparation method of the present application can prepare a Cr3C2 / 25NiCr wear-resistant coating with higher hardness, better fracture toughness and wear resistance. It should be understood that the application of the present application is not limited to the above examples. For ordinary technicians in this field, they can be improved or transformed according to the above description, and all these improvements and transformations should belong to the protection scope of the present application.

Claims

1. A method for preparing a Cr3C2 / 25NiCr wear-resistant coating, characterized in that: The following steps are involved: The Cr3C2 / 25NiCr wear-resistant coating is prepared on the surface of the substrate by explosion spraying; The fuel gas in the explosion spraying is propane, the combustion-supporting gas is oxygen, and the powder-feeding gas is hydrogen; The flow rate of the powder feeding gas is 20-40L / min; The flow rate of the fuel gas is 20-40 L / min; the flow rate of the combustion-supporting gas is 40-50 L / min; The material of the spray gun outlet section in the explosion spraying is silicon nitride; The spraying distance in the explosion spraying is 250-350 mm, the spraying angle is 90°, and the spraying speed is 4-5 mm / s; The substrate is one of Z2CN19-10 nitrogen-controlled austenitic stainless steel or Inconel 718 alloy; The oxygen-fuel ratio at the explosion center of the explosion spraying is 2.0-2.

5.

2. The method for preparing the Cr3C2 / 25NiCr wear-resistant coating according to claim 1, characterized in that: The substrate is pretreated before the explosion spraying, and the pretreatment is one or more of sandblasting, chemical cleaning and mechanical grinding; the sandblasting material is alumina sand, and the particle size of the alumina sand is 100μm; the chemical cleaning is carried out under ultrasound, and the chemical cleaning reagent is acetone.

3. The method for preparing the Cr3C2 / 25NiCr wear-resistant coating according to claim 1, characterized in that: The Cr3C2 / 25NiCr wear-resistant coating is further subjected to post-processing after preparation, and the post-processing is one of grinding, machining or polishing; after the post-processing is completed, it is also subjected to inspection, and the inspection is one or more of visual inspection, thickness gauge inspection and surface roughness instrument inspection.

4. A Cr3C2 / 25NiCr wear-resistant coating prepared by the method for preparing a Cr3C2 / 25NiCr wear-resistant coating as claimed in any one of claims 1 to 3, characterized in that: The Cr3C2 / 25NiCr wear-resistant coating has a thickness of 250-350µm, a Vickers hardness of 600-1000HV, and a fracture toughness of 4-8 MPa×m 1 / 2 , porosity ≤5%.