A high sulfur-doped porous carbon material and its preparation method and application
Through the mixing of petroleum asphalt, template agent and inorganic sulfur dopant and silane coupling agent treatment, the shortcomings in energy density and power density of lithium-ion batteries and supercapacitors are solved, and the preparation of high-sulfur doped porous carbon materials is realized. , improves electrochemical performance and stability, and reduces production costs.
Patent Information
- Application Number
- CN202311220889.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-21
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-09-21
AI Technical Summary
The existing lithium-ion batteries and supercapacitors have shortcomings in energy density and power density, and the preparation method of sulfur-doped porous carbon materials has problems such as high cost, high toxicity and limited sulfur doping, which affects the electrochemical performance of the material.
Use petroleum asphalt, template agent and inorganic sulfur dopant to mix, and after wet milling and ball milling, add silane coupling agent and hydrolyze under acidic conditions to form a highly sulfur-doped porous carbon material, which is improved by heating and boiling steps of acid solution. Sulfur doping amount and structural stability.
The preparation of porous carbon materials with high sulfur doping is achieved, which improves the electrochemical performance and structural stability of the material, reduces the preparation cost, is suitable for industrial production, has rich pore structure and good electrochemical properties.
Smart Images

Figure BDA0004460539100000071 
Figure BDA0004460539100000072 
Figure BDA0004460539100000081
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrochemical energy storage, and in particular to a sulfur-doped porous carbon material and a preparation method and application thereof. Background Art
[0002] With the depletion of fossil energy and the intensification of environmental problems, in order to ensure sustainable development, new energy has become a global hot topic. Energy storage devices including lithium-ion batteries and supercapacitors have been widely studied. Although traditional lithium-ion batteries have a high energy density, their power density is not high, which cannot meet high power output, and their cycle life is limited. Supercapacitors, as a new type of green energy storage device between traditional capacitors and batteries, have very high power density and long cycle life, but their energy density is low and cannot meet the requirements. In order to better play the advantages of each and make up for their shortcomings, researchers have tried to combine lithium-ion batteries with supercapacitors in recent years to develop a new electrochemical energy storage device-lithium-ion capacitors.
[0003] The positive electrode material of lithium-ion capacitors is mainly activated carbon, and its negative electrode material is also often made of carbon materials. In order to improve the electrochemical performance, multidimensional and complex porous carbon materials are often used as negative electrodes. The pores of multidimensional and complex porous carbon materials can provide effective diffusion channels and shorter lithium ion diffusion distances for lithium ions. The mechanical stress of volume expansion / contraction during lithium deintercalation is small, which is conducive to improving cycle stability. However, when the carbon material has more pores or uneven distribution, its structural stability will deteriorate, which may lead to poor cycle stability.
[0004] In order to further improve the electrochemical properties of carbon materials, heteroatom doping technology is also used. The introduction of sulfur atoms can not only effectively improve the conductivity and wettability of porous carbon materials and increase the interlayer spacing, but also introduce pseudocapacitance through redox reactions to increase the overall capacity. For the preparation of sulfur-doped porous carbon materials, most of them use sulfur-containing organic matter as the sulfur source. For example, Chinese patent applications CN108565462A, CN109830378A, CN112320784A and CN109704307A all use organic sulfur sources. However, in addition to being expensive and highly toxic, this type of method also has a very limited sulfur doping amount (1.5-8.0wt%), and a lower sulfur doping amount is not conducive to the high capacity and high rate performance of porous carbon materials. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a sulfur-doped porous carbon material and a preparation method and application thereof, which can increase the sulfur doping amount, ensure the stability of the porous carbon material, and better exert its electrochemical performance. The specific technical solution is as follows:
[0006] The first aspect of the present invention provides a method for preparing a highly sulfur-doped porous carbon material, comprising:
[0007] (1) mixing petroleum asphalt, a template agent, and an inorganic sulfur dopant to obtain a mixed material, and sequentially adding a wet grinding medium and a dispersant to the mixed material for ball milling to obtain a slurry;
[0008] (2) heating the slurry, then maintaining the temperature, and then cooling it to room temperature to obtain a product;
[0009] (3) adding a silane coupling agent to the product, soaking it in an acid solution and then drying it, then washing the obtained product and boiling it in an acid solution;
[0010] (4) Washing and drying the material obtained in step (3) to obtain a sulfur-doped porous carbon material.
[0011] Specifically, the mass ratio of petroleum asphalt, template and inorganic sulfur dopant in step (1) is 1:(2-4):(1-2);
[0012] Specifically, in step (1), the template agent is a carbonate selected from at least one of calcium carbonate, manganese carbonate, magnesium carbonate and sodium carbonate; the carbonate decomposes at high temperature to produce metal oxides and CO 2 The metal oxides retained in the pores can play the role of template pore formation, and the generated CO 2 Gas can also act as a physical activator, etching the carbon skeleton and promoting the formation of pore structure, ultimately forming a rich pore structure;
[0013] Specifically, in step (1), the inorganic sulfur dopant is selected from one of manganese sulfate, magnesium sulfate, calcium sulfate and zinc sulfate; after high-temperature sintering, the sulfur element in the inorganic sulfur dopant forms a C-S bond inside the sulfur-doped porous carbon, and mainly exists in the form of thiophene sulfur (CSC) and oxidized sulfur (C-SOx-C, x=2-4);
[0014] Specifically, the wet grinding medium in step (1) is an organic solvent, selected from at least one of methanol, ethanol and acetone, and the amount of wet grinding medium added in step (1) is: 1L of wet grinding medium is added for every 1-2kg of the mixed material;
[0015] Specifically, the dispersant in step (1) is at least one of citric acid, hexadecyltrimethylammonium bromide, methacrylic acid amine, polyvinylpyrrolidone and sodium dodecylsulfonate, and the amount of the dispersant added in step (1) is 0.4-0.7% of the mass of the mixed material in step (1);
[0016] Specifically, the ball milling speed in step (1) is 1400-1600 rpm, and the ball milling time is 10-15 h;
[0017] More specifically, the process of adding dispersants, wet grinding media and ball milling at a certain rotation speed is to activate the raw materials, which helps to form pores and increase the doping amount of sulfur.
[0018] Specifically, the heating temperature in step (2) is 700-1000° C., the heating rate is 2-10° C. / min, and the insulation time is 1-3 hours. During the heating process, a too fast heating rate may cause the pore structure to collapse.
[0019] Specifically, the silane coupling agent in step (3) is at least one of kh550 and kh560. The silane coupling agent can cross-link with a small amount of hydroxyl groups on the surface of the inorganic material or form a molecular layer on the surface of the inorganic material through self-cross-linking, thereby enhancing the strength and water resistance of the inorganic material.
[0020] Specifically, the amount of the silane coupling agent added in step (3) is 0.5-3% of the total mass of the petroleum asphalt and the inorganic sulfur dopant; the silane coupling agent should be added in an appropriate amount, and adding too much will affect the electrochemical properties of the material;
[0021] Specifically, the acid solution in step (3) is selected from one or more of hydrochloric acid, sulfuric acid and nitric acid solutions, and the soaking time is 3 to 6 hours;
[0022] Specifically, the drying temperature in step (3) is 50 to 60° C., and the drying time is 4 to 10 hours;
[0023] Specifically, the boiling time in step (3) is 2 to 5 hours, and the purpose of boiling in acid is to remove the template.
[0024] Specifically, the washing reagent in step (4) is deionized water or anhydrous ethanol;
[0025] Specifically, the drying temperature in step (4) is 60 to 80° C., and the drying time is 12 to 16 hours.
[0026] The second aspect of the present invention provides a highly sulfur-doped porous carbon material prepared by any of the methods described above.
[0027] The third aspect of the present invention provides a highly sulfur-doped porous carbon material prepared by any of the methods described above for use in a capacitor negative electrode.
[0028] The method for preparing the capacitor negative electrode comprises:
[0029] Step 1) mixing the above-mentioned high-sulfur-doped porous carbon material, conductive agent and binder in a mass ratio of 7-8:1:1-2, adding nitrogen methyl pyrrolidone (NMP) and stirring evenly to form a slurry;
[0030] Step 2) The slurry is evenly coated on the copper foil with a scraper, and after vacuum drying, it is punched into electrode discs, and after compaction, the negative electrode of the lithium ion capacitor is obtained.
[0031] The conductive agent in step 1) is one or more of acetylene black, carbon nanotubes, and graphene;
[0032] In step 1), the binder is one or more of polyvinylidene fluoride and polytetrafluoroethylene;
[0033] In step 1), the amount of nitrogen methyl pyrrolidone added is 45% to 55% of the total mass of the slurry;
[0034] In step 2), the drying temperature is 60 to 80° C. and the drying time is 10 to 16 hours.
[0035] When preparing the sulfur-doped porous carbon material, the present invention first adds a dispersant and a wet grinding medium for ball milling, which can make the petroleum asphalt, the template agent and the inorganic sulfur dopant more evenly dispersed, so that the petroleum asphalt, the template agent and the inorganic sulfur dopant are fully in contact, and on the other hand, the raw materials can be activated to improve the activity of the inorganic sulfur source and the carbon source, thereby improving the pore-forming effect and the sulfur doping amount;
[0036] In addition, the silane coupling agent added in the present invention is hydrolyzed under acidic conditions and cross-linked on the surface of the sulfur-doped porous carbon material to form a molecular layer, which can fix sulfur, reduce sulfur loss caused by the pickling process, and increase the sulfur content of the porous carbon material; and the molecular layer can improve the stability of the doped porous carbon material, so that it maintains a stable structure, which is more conducive to exerting better electrochemical properties.
[0037] The beneficial effects of the technical solution of the present invention are as follows:
[0038] (1) The sulfur-doped porous carbon material provided by the present invention has a rich pore structure and a high sulfur doping amount. As a negative electrode of a lithium ion capacitor, it has good electrochemical properties and has good application prospects as a negative electrode of a capacitor;
[0039] (2) The sulfur-doped porous carbon material provided by the present invention has a low preparation cost, a safe and environmentally friendly preparation process, and is conducive to realizing industrial large-scale production. DETAILED DESCRIPTION
[0040] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the present application will be clearly and completely described in combination with the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0041] Example 1
[0042] In this embodiment, the mass ratio of petroleum asphalt, template agent and inorganic sulfur dopant is 1:3:1, the amount of dispersant added is 0.5% of the mass of the mixed material, and the amount of silane coupling agent added is 2% of the total mass of petroleum asphalt and inorganic sulfur dopant. The specific method is as follows:
[0043] (1) 100 g of petroleum asphalt, 300 g of magnesium carbonate and 100 g of manganese sulfate were mixed evenly, and then 0.5 L of ethanol and 2.5 g of citric acid were added in sequence and ball milled at a speed of 1500 rpm, and then the obtained material was dried at 80°C;
[0044] (2) In a nitrogen atmosphere, the material obtained in step (1) was heated to 900° C. at a heating rate of 5° C. / min, kept at this temperature for 2 h, and then naturally cooled to room temperature to obtain a product;
[0045] (3) Add 4 g of KH560 to the product obtained in step (2), soak it in a hydrochloric acid solution with a pH of 4, and then dry it at 60°C for 8 hours. Then add a hydrochloric acid solution (V 37%浓盐酸 :V 去离子水 =1:3) and boil for 3 hours;
[0046] (4) Finally, the product obtained in step (3) was repeatedly washed with anhydrous ethanol, and then dried at 80° C. for 12 h to obtain a sulfur-doped porous carbon material.
[0047] Example 2
[0048] In this embodiment, the mass ratio of petroleum asphalt, template agent and inorganic sulfur dopant is 1:3:2, the amount of dispersant added is 0.5% of the mass of the mixture, and the amount of silane coupling agent added is 2% of the total mass of petroleum asphalt and inorganic sulfur dopant. Other features are the same as those in Example 1.
[0049] Example 3
[0050] In this embodiment, the mass ratio of petroleum asphalt, template and inorganic sulfur dopant is 1:3:1.5, the amount of dispersant added is 0.5% of the mass of the mixture, and the amount of silane coupling agent added is 2% of the total mass of petroleum asphalt and inorganic sulfur dopant. Other features are the same as those in Example 1.
[0051] Example 4
[0052] In this embodiment, the mass ratio of petroleum asphalt, template agent and inorganic sulfur dopant is 1:3:1, the amount of dispersant added is 0.5% of the mass of the mixture, and the amount of silane coupling agent added is 0.5% of the total mass of petroleum asphalt and inorganic sulfur dopant. Other features are the same as those in Example 1.
[0053] Example 5
[0054] In this embodiment, the mass ratio of petroleum asphalt, template agent and inorganic sulfur dopant is 1:3:1.5, the amount of dispersant added is 0.5% of the mass of the mixture, and the amount of silane coupling agent added is 3% of the total mass of petroleum asphalt and inorganic sulfur dopant. Other features are the same as those in Example 1.
[0055] Comparative Example 1
[0056] (1) 100 g of petroleum asphalt, 300 g of magnesium carbonate, 100 g of manganese sulfate and 2.5 g of citric acid were mixed evenly, and then the resulting material was dried at 80° C.;
[0057] (2) In a nitrogen atmosphere, the material obtained in step (1) was heated to 900° C. at a heating rate of 5° C. / min, kept at this temperature for 2 h, and then naturally cooled to room temperature to obtain a product;
[0058] (3) Add 4 g of KH560 to the initial product obtained in step (2), soak it in a hydrochloric acid solution with a pH of 4, and then dry it at 60°C for 8 hours. Then add a hydrochloric acid solution (V 37%浓盐酸 :V 去离子水 =1:3) and boil for 3 hours;
[0059] (4) Finally, the product obtained in step (3) was repeatedly washed with anhydrous ethanol, and then dried at 80° C. for 12 h to obtain a sulfur-doped porous carbon material.
[0060] Comparative Example 2
[0061] (1) 100 g of petroleum asphalt, 300 g of magnesium carbonate and 100 g of manganese sulfate were mixed evenly, and then 0.5 L of ethanol and 2.5 g of citric acid were added in sequence and ball milled at a speed of 1500 rpm, and then the obtained material was dried at 80°C;
[0062] (2) In a nitrogen atmosphere, the material obtained in step (1) was heated to 900° C. at a heating rate of 5° C. / min, kept at this temperature for 2 h, and then naturally cooled to room temperature to obtain a product;
[0063] (3) Add hydrochloric acid solution (V) to the product 37%浓盐酸 :V 去离子水 =1:3) and boil for 3 hours;
[0064] (4) Finally, the product obtained in step (3) was repeatedly washed with anhydrous ethanol, and then dried at 80° C. for 12 h to obtain a sulfur-doped porous carbon material.
[0065] Test Results
[0066] Table 1
[0067]
[0068] The results in Table 1 show that the sulfur-doped porous carbon material prepared by the method of the present invention has a rich pore structure and a high sulfur content. In Comparative Example 1, since the raw material was not properly activated, the pore-forming effect was significantly weakened and the sulfur doping amount was also reduced; in Comparative Example 2, no silane coupling agent was added to fix the doped sulfur, and the sulfur was reduced during the pickling process, and the final sulfur content was low.
[0069] Table 2
[0070]
[0071]
[0072] The test results in Table 2 show that the sulfur-doped porous carbon material prepared by the method of the present invention has a higher sulfur content and better structural stability, thus having better electrochemical performance; while the sulfur-doped porous carbon material prepared in Comparative Example 1 has a relatively smaller pore structure and less doped sulfur, resulting in poor electrochemical performance; the sulfur-doped porous carbon material prepared in Comparative Example 2 has a lower sulfur content and poorer structural stability, resulting in relatively poor electrochemical performance.
Claims
1. A method for preparing a highly sulfur-doped porous carbon material, characterized in that: include: (1) petroleum asphalt, a template agent, and an inorganic sulfur dopant are mixed uniformly to obtain a mixture, and a wet grinding medium and a dispersant are sequentially added to the mixture for ball milling to obtain a slurry; (2) heating the slurry and then keeping it warm, and then cooling it to room temperature to obtain a product; (3) adding a silane coupling agent to the product, soaking it in an acid solution, and then drying it; then washing the resulting product and boiling it in an acid solution; (4) washing and drying the material obtained in step (3) to obtain a sulfur-doped porous carbon material; The inorganic sulfur dopant in step (1) is selected from at least one of manganese sulfate, magnesium sulfate, calcium sulfate and zinc sulfate; The heating temperature in step (2) is 700-1000°C.
2. The method for preparing a highly sulfur-doped porous carbon material according to claim 1, wherein: The mass ratio of the petroleum asphalt, the template and the inorganic sulfur dopant in step (1) is 1:(2-4):(1-2).
3. The method for preparing a highly sulfur-doped porous carbon material according to claim 1, wherein: The amount of the wet grinding medium added in step (1) is: 1 L of wet grinding medium is added for every 1 to 2 kg of the mixed material.
4. The method for preparing a highly sulfur-doped porous carbon material according to claim 1, wherein: The amount of the dispersant added in step (1) is 0.4 to 0.7% of the mass of the mixed material.
5. The method for preparing a highly sulfur-doped porous carbon material according to claim 1, wherein: The ball milling speed in step (1) is 1400-1600 rpm, and the ball milling time is 10-15 h.
6. The method for preparing a highly sulfur-doped porous carbon material according to claim 1, wherein: The heating rate during the heating in step (2) is 2 to 10°C / min, and the insulation time is 1 to 3 hours.
7. The method for preparing a highly sulfur-doped porous carbon material according to claim 1, wherein: The amount of the silane coupling agent added in step (3) is 0.5 to 3% of the total mass of the petroleum asphalt and the inorganic sulfur dopant.
8. A highly sulfur-doped porous carbon material prepared by the method according to any one of claims 1 to 7.
9. A highly sulfur-doped porous carbon material prepared by the method according to any one of claims 1 to 7 and used for a capacitor negative electrode.