Photovoltaic module recycling equipment and method based on supercritical foaming technology
Supercritical foaming technology is used in photovoltaic module recycling equipment to foam the adhesive layer of waste photovoltaic modules in a supercritical state. This solves the problems of low recovery rate and long time consumption in the existing technology and achieves efficient photovoltaic module separation. and recycling, improving the recycling speed and rate.
Patent Information
- Application Number
- CN202311482853.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2023-07-14
- Filing Date
- 2023-11-08
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2043-11-08
AI Technical Summary
Among the existing photovoltaic module recycling technologies, the incineration method results in low recovery rate and high loss, while the acid solution dissolution method is time-consuming and slow in recovery speed, making it impossible to fully recycle valuable materials.
Photovoltaic module recycling equipment and methods based on supercritical foaming technology are used to foam the waste photovoltaic modules in a supercritical state through the foaming unit, and then cool down to separate the silicon wafers, solder ribbons, backsheets and glass to achieve automation Separation and packaging.
It improves the recovery speed and recovery rate of photovoltaic modules, reduces material loss, avoids the use of acidic solutions, and achieves the complete recovery of silicon wafers, backsheets and glass.
Smart Images

Figure CN117299738B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of photovoltaic module recycling, and specifically relates to a photovoltaic module recycling device based on supercritical foaming technology. The present invention also relates to a photovoltaic module recycling method based on supercritical foaming technology. Background Art
[0002] Photovoltaic modules are devices that can convert solar energy into electrical energy, including packaging materials (frames, junction boxes, cables) and laminates stacked from bottom to top (backplane or glass substrate, organic adhesive layer, battery layer, organic adhesive layer, glass substrate. Except for the organic adhesive layer, most of the components such as silicon, aluminum, silver, and glass in the packaging materials and laminates can be recycled and reused. As the operating time increases, the power generation efficiency of photovoltaic modules gradually decreases. In order to achieve better power generation performance, old photovoltaic modules need to be replaced. Recycling discarded photovoltaic modules can not only protect the environment but also effectively save resources.
[0003] At present, physical separation methods are mostly used for recycling photovoltaic modules. The disassembly of aluminum frames, glass and junction boxes is mostly done manually to obtain frameless modules, which is time-consuming, labor-intensive, and dusty and harmful to workers' health. For frameless modules, one method is to use an incinerator to burn the crushed photovoltaic modules, so as to separate and recycle the cells, glass and welding strips. The products obtained are crushed glass and broken cells, which are difficult to screen and separate, wasting a lot of manpower and material costs. In addition, there is a large loss of materials during separation, and the valuable materials cannot be fully recycled. Another method is to place the photovoltaic modules in a container containing an inorganic acid or organic acid solution to dissolve the organic adhesive film in the photovoltaic modules, so as to separate the cells from the glass. The recycling cycle is relatively long, requiring more than one week, and the waste liquid is difficult to treat in the later stage.
[0004] Therefore, how to solve the above technical problems should be the focus of technical personnel in this field. The purpose of the present invention is to provide a photovoltaic module recycling equipment and method based on supercritical foaming technology, to provide automated technical support for the photovoltaic module recycling industry, and to improve the recycling speed and recovery rate of photovoltaic modules. Summary of the invention
[0005] The purpose of the present invention is to provide a photovoltaic module recycling device based on supercritical foaming technology, which solves the problems of low recovery rate and high loss caused by the incineration method in the prior art and long time consumption and slow recovery speed caused by the acid solution dissolution method.
[0006] Another object of the present invention is to provide a photovoltaic module recycling method based on supercritical foaming technology.
[0007] The first technical solution adopted by the present invention is: photovoltaic module recovery equipment based on supercritical foaming technology, including a foaming unit, the inlet end of the foaming unit is connected to the encapsulation dissociation unit, the outlet end of the foaming unit is connected to the cooling unit and the subpackaging unit in sequence, the foaming unit includes a reactor cabin, the reactor cabin is provided with a heating device, the outside of the reactor cabin is connected to a foaming gas injection device through a pipeline, and a booster device is provided on the connecting pipeline.
[0008] The first technical solution of the present invention is also characterized in that:
[0009] The foaming unit also includes a feeding platform connected to the inlet of the reactor cabin, a discharging platform connected to the outlet of the reactor cabin, and a circulating fan arranged in the reactor cabin.
[0010] The packaging dissociation unit comprises a wire box and cable removal mechanism connected to the feeding platform, and the other end of the wire box and cable removal mechanism is connected to the short frame removal mechanism, the long frame removal mechanism and the input mechanism in sequence.
[0011] The cooling unit comprises an output mechanism connected with the discharging platform, the other end of the output mechanism is connected with a temperature control cabin, and a cooling device is arranged in the temperature control cabin.
[0012] The subpackaging unit comprises a feeding platform connected with the temperature-controlled cabin, and the other end of the feeding platform is connected with a sorting mechanism and a packaging mechanism in sequence.
[0013] The second technical solution adopted by the present invention is: a photovoltaic module recycling method based on supercritical foaming technology, comprising the following steps:
[0014] Step 1: Send the waste photovoltaic modules to the packaging and dissociation unit, remove the frames, junction boxes and cables of the waste photovoltaic modules to obtain frameless photovoltaic modules;
[0015] Step 2, the frameless photovoltaic module is sent into the reactor cabin of the foaming unit, the heating device controls the temperature in the reactor cabin to a set temperature, the foaming gas injection device injects foaming gas into the reactor cabin and pressurizes it to a set pressure through the booster device to make the foaming gas in the reactor cabin enter a supercritical state, and after the supercritical foaming gas and the adhesive layer of the frameless photovoltaic module are fully foamed, a photovoltaic module with a foamed adhesive layer is obtained;
[0016] Step 3, sending the photovoltaic module after the foaming of the adhesive layer into a cooling unit to be cooled step by step to room temperature, so as to obtain silicon wafers, welding strips, backplanes and glass separated from each other;
[0017] Step 4: Send the product obtained in step 3 to a subpackaging unit to sort out silicon wafers, solder strips, backplanes, and glass, and then package them separately.
[0018] The second technical solution of the present invention is also characterized in that:
[0019] The set temperature in step 2 is 50-300° C., preferably 80° C.; the set pressure is 5-30 MPa, preferably 14 MPa; and the foaming reaction time is 0.5-2 h, preferably 1 h.
[0020] The foaming gas is CO2, or the foaming gas is one or a mixture of two or more inert gases.
[0021] The cooling method in step 3 is water circulation cooling or ice making cooling, and the temperature drops to room temperature within 5 to 15 minutes.
[0022] The beneficial effects of the present invention are as follows: the photovoltaic module recycling equipment and method based on supercritical foaming technology of the present invention obtains the photovoltaic module after the glue layer is foamed by fully reacting the supercritical foaming gas with the glue layer of the frameless photovoltaic module, and performs temperature control and cooling treatment on the photovoltaic module after the glue layer is foamed to obtain silicon wafers, welding strips, back panels and glass separated from each other, thereby realizing the separation and recycling of photovoltaic modules, and the silicon wafers, back panels and glass can all achieve integrity, with less loss and high recovery rate, without the need to use acidic solution for dissolution, thereby improving the recovery speed. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic structural diagram of a photovoltaic module recycling device based on supercritical foaming technology of the present invention;
[0024] Figure 2 It is a schematic flow chart of the photovoltaic module recycling method based on supercritical foaming technology of the present invention.
[0025] In the figure, 1. encapsulation and dissociation unit, 2. foaming unit, 3. cooling unit, 4. subpackaging unit;
[0026] 11. Input mechanism, 12. Long frame removal mechanism, 13. Short frame removal mechanism, 14. Wire box and cable removal mechanism;
[0027] 21. Reactor cabin, 22. Heating device, 23. Foaming gas injection device, 24. Pressurizing device, 25. Feeding platform, 26. Discharging platform;
[0028] 31. Output mechanism, 32. Temperature control cabin, 33. Cooling device;
[0029] 41. Feeding platform, 42. Sorting mechanism, 43. Packing mechanism. DETAILED DESCRIPTION
[0030] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0031] Example 1
[0032] The present invention provides a photovoltaic module recycling device based on supercritical foaming technology, such as Figure 1 As shown, it includes an encapsulation and dissociation unit 1, a foaming unit 2, a cooling unit 3 and a subpackaging unit 4 which are connected in sequence. Among them, the encapsulation and dissociation unit 1 includes an input mechanism 11, a long frame removal mechanism 12, a short frame removal mechanism 13, and a wire box and cable removal mechanism 14 which are connected in sequence; the foaming unit 2 includes a reactor cabin 21, a feeding platform 25 connected to the inlet of the reactor cabin 21, and a discharging platform 26 connected to the outlet of the reactor cabin 21, the other end of the feeding platform 25 is connected to the wire box and cable removal mechanism 14, and a heating device 22 and a high-pressure circulation fan are arranged in the reactor cabin 21 to circulate the foaming gas in the reactor cabin 21. A ring is provided to ensure that all components in all positions of the entire kettle can undergo foaming reaction. A foaming gas injection device 23 is connected to the outside of the reactor chamber 21 through a pipeline, and a booster device 24 is arranged on the connecting pipeline; the cooling unit 3 comprises an output mechanism 31 connected to the discharge platform 26, and the other end of the output mechanism 31 is connected to a temperature control chamber 32, and a cooling device 33 is arranged in the temperature control chamber 32; the subpackaging unit 4 comprises a feeding platform 41 connected to the temperature control chamber 32, and the other end of the feeding platform 41 is connected to a sorting mechanism 42 and a packaging mechanism 43 in sequence.
[0033] Example 2
[0034] When the photovoltaic module recycling equipment of the present invention is installed, the long frame removal mechanism 12 and the short frame removal mechanism 13 adopt a photovoltaic panel frame removal device previously developed by the applicant (publication number: CN215201862U, CN112497165A); the wire box cable removal mechanism 14 adopts a device for cutting the wire box cable of the photovoltaic panel previously developed by the applicant (publication number: CN214639875U). The reactor cabin 21 and the heating device 22 directly adopt the existing conventional heating reactor; the foaming gas injection device 23 adopts the model YZPR-100 of Yanzheng Instrument; the booster device 24 adopts a compressor with a discharge regulating valve. The temperature control cabin 32 adopts the existing conventional insulation cabin; the cooling device 33 adopts the existing refrigeration device. The sorting mechanism 42 adopts the photovoltaic module intermediate material recovery device based on the electrostatic sorting principle (publication number: CN114669397A) or the photovoltaic module recovery intermediate material sorting equipment based on the excitation force (publication number: CN114733769A) developed by the affiliated unit of the same actual controller of the applicant; the packaging mechanism 43 adopts the belt structure automatic quantitative packaging machine (product model: WMD180-PDJG) of Xuzhou Womedno Machinery; the remaining input mechanism 11, feeding platform 25, discharging platform 26, output mechanism 31, and feeding platform 41 can all adopt existing conventional conveyor belts. The injection gas of the foaming gas injection device 23 of the present invention is preferably but not limited to CO2 or N2 or other gases (various inert gases with similar properties) used alone or in combination for supercritical foaming.
[0035] Example 3
[0036] Photovoltaic module recycling methods based on supercritical foaming technology, such as Figure 2 As shown, the following steps are included:
[0037] Step 1: Send the waste photovoltaic modules into the packaging and dissociation unit 1 through the input mechanism 11, remove the frames of the waste photovoltaic modules through the long frame removal mechanism 12 and the short frame removal mechanism 13, and obtain frameless photovoltaic modules after the junction box and cables are removed through the junction box and cable removal mechanism 14.
[0038] Step 2, the frameless photovoltaic module is sent into the reactor cabin 21 of the foaming unit 2 through the feeding platform 25, the heating device 22 controls the temperature in the reactor cabin 21 to 50-300°C, the foaming gas injection device 23 injects CO2 into the reactor cabin 21 and pressurizes it to 5-30MPa through the booster device 24 to make the CO2 in the reactor cabin 21 enter a supercritical state, the supercritical CO2 is affected by the temperature in the reactor cabin 21, and evaporates rapidly to form bubbles, so that the adhesive layer material produces a large number of pores and volume expansion, thereby achieving the purpose of foaming, after the supercritical CO2 and the adhesive layer of the frameless photovoltaic module are foamed for 0.5-2h, that is, the adhesive layer located at the center of the plane is also fully reacted, the photovoltaic module with the foamed adhesive layer is sent out through the discharging platform 26, at this time, the adhesive layer and the silicon wafers, welding strips, backplanes or glass on both sides have been peeled off in a honeycomb-like state but not completely peeled off.
[0039] Step 3, the photovoltaic module after the foaming of the adhesive layer is sent into the temperature control chamber 32 of the cooling unit 3 through the output mechanism 31. The temperature control chamber 32 is provided with a cooling device 33, so that the photovoltaic module is gradually cooled to room temperature within 5 to 15 minutes to prevent the glass in the photovoltaic module from being suddenly cooled and broken. At the same time, the foamed adhesive layer shrinks due to the cold and is completely peeled off from the silicon wafers, welding strips, backplanes or glass on both sides thereof, so as to obtain silicon wafers, welding strips, backplanes and glass separated from each other.
[0040] Step 4, the product obtained in step 3 is sent to the subpackaging unit 4 via the feeding platform 41, and the silicon wafers, solder strips, backplanes and glass are respectively sorted out by the sorting mechanism 42, and then they are separately packaged by the packaging mechanism 43.
[0041] Results Analysis
[0042] 1. Preparation before the experiment
[0043] Experimental materials: retired photovoltaic panels (without frame, junction box, or cable)
[0044] Experimental samples: photovoltaic modules of different models and types (divided into 60*30mm small pieces);
[0045] Other variables are: 1. Sample model and type; 2. Pressure; 3. Temperature; 4. Reaction time;
[0046] Experimental equipment: Foaming unit - supercritical CO2 foaming reactor (the reactor used in the experiment is 100ml specification)
[0047] Reactor size:
[0048] 2. Experimental Records
[0049] No.: 1
[0050] Test time: 2023.7.24
[0051] Foaming temperature: 75℃; Pressure: 9Mpa;
[0052] Test sample: 60*30mm small piece;
[0053] Test results:
[0054] ① Sample 1 (pressure holding time: 30min):
[0055] There is obvious bubbling, the glass is partially peeled off, and the back panel can be manually torn off with a certain amount of force and angle;
[0056] ② Sample 2 (pressure holding time: 60min):
[0057] There is obvious bubbling, the glass is partially peeled off, and the back panel can be torn off manually;
[0058] ③Sample 3 (pressure holding time: 90min):
[0059] There is obvious bubbling, most of the glass has fallen off, and the back panel can be torn off manually;
[0060] ④ Sample 4 (pressure holding time: 120min):
[0061] There is obvious bubbling, most of the glass has fallen off, and the back panel is partially separated and can be torn off manually;
[0062] No.: 2
[0063] Test time: 2023.7.24
[0064] Foaming temperature: 75℃; pressure: 5Mpa; holding time: 60min;
[0065] Test sample: 60*30mm small piece;
[0066] Test results:
[0067] ①Sample 1:
[0068] There is no obvious bubbling, the glass partially falls off, and the back panel can be partially torn off manually;
[0069] ②Sample 2:
[0070] There is bubbling, the glass is partially peeled off, and the back panel can be partially torn off manually;
[0071] No.: 3
[0072] Test time: 2023.7.24
[0073] Foaming temperature: 75℃; pressure: 8Mpa; holding time: 60min;
[0074] Test sample: 60*30mm small piece;
[0075] Test results:
[0076] ①Sample 1:
[0077] There is bubbling, the glass partially falls off, and the back panel can be torn off manually;
[0078] ②Sample 2:
[0079] There is obvious foaming, and the back panel can be torn off manually;
[0080] No.: 4
[0081] Test time: 2023.7.24
[0082] Foaming temperature: 75℃; pressure: 11Mpa; holding time: 60min;
[0083] Test sample: 60*30mm small piece;
[0084] Test results:
[0085] ①Sample 1:
[0086] There is obvious bubbling, the glass is partially peeled off, and the back panel can be torn off manually;
[0087] ②Sample 2:
[0088] There is obvious foaming, and the back panel is partially detached, which can be partially torn off manually;
[0089] No.: 5
[0090] Test time: 2023.7.24
[0091] Foaming temperature: 75℃; pressure: 15Mpa; holding time: 60min;
[0092] Test sample: 60*30mm small piece;
[0093] Test results:
[0094] ①Sample 1:
[0095] There is obvious bubbling, most of the glass has fallen off, and the back panel can be torn off manually;
[0096] ②Sample 2:
[0097] There is obvious foaming, and the back panel is partially detached, which can be partially torn off manually;
[0098] No.: 6
[0099] Test time: 2023.7.24
[0100] Foaming temperature: 75℃; pressure: 21Mpa; holding time: 60min;
[0101] Test sample: 60*30mm small piece;
[0102] Test results:
[0103] ①Sample 1:
[0104] There is obvious bubbling, the glass is falling off, and the back panel can be torn off manually;
[0105] ②Sample 2:
[0106] There is obvious foaming, the back panel is partially detached, and the remaining part can be torn off;
[0107] No.: 7
[0108] Test time: 2023.7.24
[0109] Foaming temperature: 75℃; pressure: 30Mpa; holding time: 60min;
[0110] Test sample: 60*30mm small piece;
[0111] Test results:
[0112] ①Sample 1:
[0113] There is bubbling, most of the glass has fallen off, and the back panel can be torn off manually;
[0114] ②Sample 2:
[0115] There is foaming, and the back panel is difficult to tear off;
[0116] No.: 8
[0117] Testing time: 2023.10.25
[0118] Foaming temperature: 50℃; pressure: 16Mpa; holding time: 60min;
[0119] Test sample: 60*30mm small piece;
[0120] Test results:
[0121] ①Sample 1:
[0122] There is no obvious bubbling in the adhesive layer; the thin layer near the glass side is not separated and cannot be torn off; there is no separation between the silicon wafer layer and the edge of the adhesive layer, making it difficult to tear off manually; the glass does not detach automatically and cannot be peeled off manually;
[0123] ②Sample 2:
[0124] There is no bubbling in the adhesive layer; there is no separation between the silicon wafer layer and the adhesive layer, and they cannot be torn apart manually; the glass does not detach automatically, and the part cannot be peeled off manually;
[0125] No.: 9
[0126] Testing time: 2023.10.25
[0127] Foaming temperature: 80℃; pressure: 14Mpa; holding time: 60min;
[0128] Test sample: 60*30mm small piece;
[0129] Test results:
[0130] ①Sample 1:
[0131] The adhesive layer has obvious foaming phenomenon; the back panel automatically separates (bubbles appear in the adhesive layer on the back); the thin layer close to the glass side can be manually torn off (no bubbles in the adhesive layer); the silicon wafer layer and the three sides of the adhesive layer are separated, about 1 to 5 mm, and can be manually torn off; most of the glass automatically detaches, about 2 / 3 to 3 / 4, and can be peeled off manually with slight force;
[0132] ②Sample 2:
[0133] The adhesive layer has obvious foaming phenomenon; the back panel does not separate automatically, but can be torn off manually; there is a separation phenomenon between the silicon layer and one side of the adhesive layer (close to the glass side), about 5 to 8 mm, which can be torn off manually; most of the glass is automatically separated, and a few pieces are left, which can be peeled off manually with a little force;
[0134] No.: 10
[0135] Testing time: 2023.10.25
[0136] Foaming temperature: 100℃; pressure: 16Mpa; holding time: 45min;
[0137] Test sample: 60*30mm
[0138] Test results:
[0139] ①Sample 1:
[0140] The adhesive layer has foaming phenomenon; the back panel has not been separated and can be torn off manually; the silicon layer and the adhesive layer at the four corners are separated; the glass has not been separated automatically and can be peeled off manually with a certain force and angle;
[0141] ②Sample 2:
[0142] The adhesive layer has foaming phenomenon; the back panel has not been separated, and there is a slight separation phenomenon at the two corners that cannot be torn apart; there is no separation phenomenon between the silicon layer and the adhesive layer at the four corners; the glass part automatically detaches, about 1 / 3, and can be peeled off manually with slight force and angle;
[0143] No.: 11
[0144] Test time: 2023.10.26
[0145] Foaming temperature: 150℃; pressure: 10Mpa; holding time: 60min;
[0146] Test sample: 60*30mm small piece;
[0147] Test results:
[0148] ①Sample 1:
[0149] The adhesive layer has foaming phenomenon; the back panel has not been separated and is difficult to tear off manually; the silicon layer on the three sides is slightly separated from the adhesive layer, about 1 to 2 mm, and it is difficult to tear off manually; the edge glass is slightly separated automatically, only one or two particles, and it requires a certain force and angle to peel manually;
[0150] ②Sample 2:
[0151] The adhesive layer has foaming phenomenon; the back panel has two edges separated, and you can try to tear it off manually; (one side is a double back panel, the part near the glass side is automatically separated, and the back side is more difficult to tear by hand); whether the silicon wafer layer and the adhesive layer are separated, and they cannot be torn apart manually; most of the glass is automatically separated, about 4 / 5 to 7 / 8, and the remaining part can be peeled off manually with slight force and angle;
[0152] No.: 12
[0153] Test time: 2023.10.26
[0154] Foaming temperature: 200℃; pressure: 12Mpa; holding time: 60min;
[0155] Test sample: 60*30mm small piece;
[0156] Test results:
[0157] ①Sample 1:
[0158] The adhesive layer has foaming phenomenon; the back panel has not been separated and is difficult to tear off manually; the silicon layer on the three sides is slightly separated from the adhesive layer, about 1 to 2 mm, and is difficult to tear off manually; the edge glass is slightly separated automatically, only one or two particles, and can only be peeled off manually with a certain force and angle;
[0159] ②Sample 2:
[0160] The adhesive layer has foaming phenomenon; the back panel has not been separated and cannot be torn off manually; there is a slight separation between the silicon layer and both sides of the adhesive layer, about 0.5-1mm, and it cannot be torn off manually; the glass part automatically detaches, about 1 / 3-1 / 2, and the remaining part can be peeled off manually with a certain force and angle;
[0161] No.: 13
[0162] Test time: 2023.10.27
[0163] Foaming temperature: 250℃; pressure: 16Mpa; holding time: 45min;
[0164] Test sample: 60*30mm small piece;
[0165] Test results:
[0166] ①Sample 1:
[0167] The adhesive layer has obvious bubbling; the back panel is not separated and is difficult to tear off manually; there is a slight separation between the silicon layer and the adhesive layer on one side, about 3mm, which is difficult to tear off manually; a small amount of glass automatically detaches, about 1 / 6 to 1 / 4, and can be peeled off manually with slight force and angle;
[0168] ②Sample 2:
[0169] The adhesive layer has foaming phenomenon; the back panel has not been separated, and one corner has slight separation phenomenon, which can be torn off manually; the silicon wafer layer and the adhesive layer have slight separation phenomenon on one side, which cannot be torn off manually; a silicon wafer automatically detaches (there is adhesive on the surface); the glass part detaches automatically, about 1 / 2 to 3 / 4, and can be peeled off manually with slight force and angle;
[0170] No.: 14
[0171] Test time: 2023.10.27
[0172] Foaming temperature: 300℃; pressure: 16Mpa; holding time: 60min;
[0173] Test sample: 60*30mm small piece;
[0174] Test results:
[0175] ①Sample 1:
[0176] The adhesive layer has foaming and the edge has melting; the back panel has not been separated and is difficult to tear off manually; the silicon layer on the three sides is slightly separated from the adhesive layer, about 1 to 2 mm, and is difficult to tear off manually; the edge glass is slightly separated automatically, about 1 / 10 to 1 / 20, and can be peeled off manually with a certain force and angle;
[0177] ②Sample 2:
[0178] The adhesive layer has foaming and the edge has melting; the back panel has not been separated and is difficult to tear off manually; the silicon wafer layer and the adhesive layer have two corners that are slightly separated and cannot be torn off manually; the glass part is automatically separated, about 1 / 3 to 1 / 2, and can be peeled off manually with slight force and angle; two pieces of solder tape / silicon wafer attached to the glass are separated;
[0179] 3. Experimental Conclusion
[0180] According to the above test results, we can see that:
[0181] ① For sample No. 1, the longer the foaming time, the more obvious the foaming effect. However, for the sake of overall production efficiency and to ensure functionality, about 1 hour is the most ideal.
[0182] ② For samples No. 2 to 7, the foaming effect is more obvious when the pressure is higher, but it will decrease after exceeding a certain value. However, in order to ensure the overall production efficiency and equipment status and reduce energy consumption, about 10Mpa is more ideal;
[0183] ③ For samples No. 8 to 14, the glass separation effect is more obvious (80℃, 14Mpa, 60min). In different temperature ranges, the test results are quite different. When the temperature is too high, the components show obvious deformation and bending, which is not conducive to subsequent work processes. When the temperature is lower than or equal to 50 degrees, there is no foaming phenomenon in the components. When the temperature is higher than or equal to 300 degrees, the components are severely deformed and the glue layer melts.
Claims
1. Photovoltaic module recycling equipment based on supercritical foaming technology, characterized in that: The invention comprises a foaming unit (2), wherein the inlet end of the foaming unit (2) is connected to a packaging dissociation unit (1) for removing frames, junction boxes and cables of discarded photovoltaic modules to obtain frameless photovoltaic modules, and the outlet end of the foaming unit (2) is connected to a cooling unit (3) and a subpackaging unit (4) in sequence, and the foaming unit (2) comprises a reactor cabin (21), a heating device (22) is arranged inside the reactor cabin (21), a foaming gas injection device (23) is connected to the outside of the reactor cabin (21) via a pipeline, and a pressurizing device (24) is arranged on the connecting pipeline, and the foaming gas injection device (23) injects foaming gas CO2 into the reactor cabin (21) and passes through the pressurizing device (24) to heat the reactor cabin (21). ) is pressurized to make CO2 enter a supercritical state, and the supercritical CO2 reacts with the adhesive layer of the frameless photovoltaic module to obtain a photovoltaic module after the adhesive layer is foamed. The foaming unit (2) also includes a feeding platform (25) connected to the inlet of the reactor cabin (21), a discharging platform (26) connected to the outlet of the reactor cabin (21), and a circulating fan arranged in the reactor cabin (21); the cooling unit (3) includes an output mechanism (31) connected to the discharging platform (26), the other end of the output mechanism (31) is connected to the temperature control cabin (32), and a cooling device (33) is arranged in the temperature control cabin (32) for gradually cooling the photovoltaic module after the adhesive layer is foamed to room temperature.
2. The photovoltaic module recycling equipment based on supercritical foaming technology according to claim 1, characterized in that: The packaging dissociation unit (1) comprises a wire box cable removal mechanism (14) connected to a feeding platform (25); the other end of the wire box cable removal mechanism (14) is sequentially connected to a short frame removal mechanism (13), a long frame removal mechanism (12) and an input mechanism (11).
3. The photovoltaic module recycling equipment based on supercritical foaming technology according to claim 1, characterized in that: The subpackaging unit (4) comprises a feeding platform (41) connected to the temperature-controlled chamber (32); the other end of the feeding platform (41) is connected in sequence to a sorting mechanism (42) and a packaging mechanism (43).
4. The recycling method of photovoltaic module recycling equipment based on supercritical foaming technology according to claim 1, characterized in that: The following steps are involved: Step 1: Send the discarded photovoltaic modules to the packaging and dissociation unit (1), remove the frames, junction boxes and cables of the discarded photovoltaic modules to obtain frameless photovoltaic modules; Step 2, the frameless photovoltaic module is sent into the reactor cabin (21) of the foaming unit (2), the temperature in the reactor cabin (21) is controlled by the heating device (22) to be 50-300° C., the foaming gas injection device (23) injects foaming gas CO2 into the reactor cabin (21) and pressurizes the CO2 in the reactor cabin (21) to 5-30 MPa through the booster device (24) so that the CO2 in the reactor cabin (21) enters a supercritical state, and the supercritical CO2 reacts with the adhesive layer of the frameless photovoltaic module for 0.5-2 hours to obtain a photovoltaic module after the adhesive layer is foamed; Step 3, sending the photovoltaic module after the foaming of the adhesive layer into the cooling unit (3) to be cooled step by step to room temperature, thereby obtaining silicon wafers, welding strips, backplanes and glass separated from each other; Step 4: Send the product obtained in step 3 to the subpackaging unit (4) to sort out the silicon wafers, solder strips, backplanes and glass, and then package them separately.
5. The photovoltaic module recycling equipment based on supercritical foaming technology according to claim 4, characterized in that: The set temperature in step 2 is 80° C., the set pressure is 14 MPa, and the foaming reaction time is 1 hour.
6. The photovoltaic module recycling equipment based on supercritical foaming technology according to claim 4, characterized in that: The cooling method in step 3 is water circulation cooling or ice making cooling, and the temperature drops to room temperature within 5 to 15 minutes.
Citation Information
Patent Citations
Photovoltaic panel frame dismantling equipment
CN112497165A
Photovoltaic module intermediate material recovery device and method based on electrostatic separation principle
CN114669397A
Device and method for sorting recycled intermediate materials of photovoltaic module based on exciting force
CN114733769A
Equipment for cutting off wire box cable of photovoltaic panel
CN214639875U
Photovoltaic panel frame dismantling equipment
CN215201862U