Electroabsorption modulator laser and preparation method thereof

By designing deep isolation trenches and window structures at the light exit end of the EAM area on both sides of the shallow ridge waveguide structure of the DFB laser, the problem of carrier injection leakage is solved, the threshold current is reduced, the output optical power of the EML laser is increased, and high efficiency is achieved anti-reflective effect.

CN117394138BActive Publication Date: 2024-10-29WUHAN YUNLING OPTOELECTRONICS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202311285162.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-07
Publication Date
2024-10-29
Estimated Expiration
2043-10-07

AI Technical Summary

Technical Problem

In integrated electroabsorption modulated lasers, the working principles of DFB lasers and EAM modulators are different, which leads to serious leakage when carriers are injected into the window structure of the DFB laser with a shallow ridge waveguide structure, resulting in an increase in threshold current and a decrease in carrier injection efficiency. , it is difficult to meet the high output power requirements.

Method used

Deep isolation trenches are designed on both sides of the shallow ridge waveguide structure of the DFB laser, and a window structure is formed at the light exit end of the EAM area. The anti-reflection solution of the deep isolation trench and window structure is combined to reduce carrier leakage and threshold current.

Benefits of technology

It effectively reduces the threshold current of the DFB laser, increases the output optical power of the EML laser, and enhances the anti-reflection capability without affecting the testing and packaging process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117394138B_ABST
    Figure CN117394138B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of chip technology, and provides a method for preparing an electro-absorption modulator laser, including S1, forming a window structure at the light-emitting end of the EAM region through masking, growth and etching; S2, then continuing masking and etching to make a deep isolation groove; S3, then opening an electric injection window after masking and etching again, wherein the EAM window structure does not open the electric injection window; S4, making electrodes in the LD region and the EAM region, wherein the EAM window structure does not make electrodes; S5, after the electrodes are made, decomposing into a single electro-absorption modulator laser chip. An electro-absorption modulator laser is also provided, including a DFB laser and an EAM electro-absorption modulator, deep isolation grooves are provided on both sides of the DFB laser ridge waveguide or isolation region, and a window structure is made at the light-emitting end of the EAM electro-absorption modulator. The present invention designs deep isolation grooves on both sides of the shallow ridge waveguide or isolation region of the DFB laser to greatly reduce the leakage at the docking interface of the docking window during the carrier injection process of the DFB laser.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chips, in particular to an electro-absorption modulator laser and a preparation method thereof. Background Art

[0002] Semiconductor lasers have the advantages of small size, light weight, low cost, and easy mass production, and have broad development prospects in the fields of optical storage, optical communication, and national defense. Among them, EML lasers integrate lasers and electro-absorption modulators on the same semiconductor chip, which has the advantages of low driving voltage, low power consumption, high modulation bandwidth, small size, and compact structure. It is more suitable for high-speed and long-distance transmission than traditional DFB lasers.

[0003] The common EML electro-absorption modulated laser is a distributed feedback DFB laser integrated with an EAM modulator to simultaneously realize the functions of light source and high-speed electro-optical modulation. In such an integrated semiconductor laser, the reflected light with the modulated signal on the laser light-emitting end face will return to the DFB area to form resonance, which will have an adverse effect on the operation of the DFB laser. With the continuous development of optical fiber networks, the power requirements for modulated lasers are becoming higher and higher. The traditional method is to plate an anti-reflection anti-reflection film on the light-emitting end of the laser to reduce the reflectivity to reduce the reflected light crosstalk. With the continuous increase in the output power of the laser, it is not enough to simply plate an anti-reflection film on the light-emitting end face to suppress the reflected light crosstalk. The usual improved approach is to optimize the waveguide structure and adopt a curved waveguide structure or a docking window structure. In essence, they all form a divergent light field at the light-emitting cavity surface to reduce the proportion of reflected light coupled back into the waveguide, thereby achieving the suppression of the reflected light crosstalk intensity. In comparison, the curved waveguide structure creates a larger angle between the chip light output and the cleavage cavity surface, which has an adverse effect on testing and packaging, especially multi-channel integrated packaging. The docking window structure can suppress the crosstalk of reflected light without affecting testing and packaging, and is a more attractive solution.

[0004] The ridge waveguide structure is a commonly used laser waveguide structure. Compared with the buried heterojunction structure, it has the characteristics of simple process technology, low cost and high reliability. In the integrated electro-absorption modulated laser, due to the different working principles of the DFB laser and the EAM modulator, a shallow ridge waveguide structure is usually used in the DFB laser area to prevent reliability risks, while a deep ridge waveguide structure is used in the EAM modulator area to reduce the intrinsic capacitance and increase the modulation bandwidth. The application of the window structure anti-reflection scheme in such a waveguide structure will cause a large amount of carrier injection of the DFB laser with a shallow ridge waveguide structure to leak to the docking interface between the window structure and the active area, causing the threshold current of the DFB laser to increase sharply and the carrier injection efficiency to drop significantly. Summary of the invention

[0005] The object of the present invention is to provide an electro-absorption modulator laser and a method for preparing the same, which can at least solve some of the defects in the prior art.

[0006] To achieve the above object, the embodiment of the present invention provides the following technical solution: a method for preparing an electro-absorption modulator laser, wherein the prepared electro-absorption modulator laser has an LD region and an EAM region, and specifically comprises the following steps:

[0007] S1, forming a window structure at the light output end of the EAM region through masking, growth and etching;

[0008] S2, then continue masking and etching to form deep isolation trenches;

[0009] S3, after masking and etching, an electric injection window is opened, wherein the EAM window structure does not have an electric injection window;

[0010] S4, making electrodes in the LD region and the EAM region, wherein the EAM window structure does not serve as an electrode;

[0011] S5, after the electrodes are fabricated, they are decomposed into a single electro-absorption modulator laser chip.

[0012] Further, in step S1, the specific production process is:

[0013] S10, growing an epitaxial structure once, and then manufacturing a grating on the epitaxial structure;

[0014] S11, performing secondary epitaxial growth of a grating buried layer on the grating;

[0015] S12, then continue to grow the mask layer, remove the mask of the EAM region, and then continue to etch the EAM region, at least etching to the buffer layer of the epitaxial structure;

[0016] S13, sequentially butt-growing an EAM active layer and an InP layer in the EAM region;

[0017] S14, growing the mask layer again, and removing the mask at the light-emitting end of the EAM region by etching, and continuing etching until at least the buffer layer is etched;

[0018] S15, growing an InP layer at the light-emitting end of the EAM region into a window structure;

[0019] S16, then grow the P-type waveguide layer and contact layer,

[0020] S17, after the growth is completed, continue masking and etching away the mask and contact layer on the EAM window structure.

[0021] Further, the specific method of making the deep isolation trench is:

[0022] After the mask is formed, etching is performed until the grating layer is etched.

[0023] Then, shallow ridge waveguides are fabricated in the LD region and the EAM region, wherein no ridge waveguide is fabricated at the light output end of the EA region.

[0024] Then, the LD region is protected, and etching is performed in the isolation region and the EAM region, at least to the buffer layer, to form a deep ridge waveguide.

[0025] The isolation region, the EAM region and a partial region of the ridge waveguide are protected to expose the middle portion of the LD region ridge waveguide groove, and then the middle region of the LD region ridge waveguide is continuously etched, at least to the buffer layer, to form a deep isolation groove.

[0026] Further, etching is performed behind the mask to protect the light-emitting end of the EAM region, and ridge waveguides are made in the LD region and the EAM region. At the same time, the region other than the ridge waveguide in the isolation region at the junction of the LD region and the EAM region is etched.

[0027] Then, the LD region is protected, the isolation region and the EAM region are exposed, and the isolation region and the region of the EAM region not protected by the mask are etched, at least to the buffer layer, to form a deep isolation trench in the isolation region.

[0028] Furthermore, in the step S3, after masking, the mask on the isolation region ridge waveguide at the junction of the LD region and the EAM region is removed by etching, and then the contact layer and the P-type waveguide layer on the surface of the isolation region ridge waveguide are removed.

[0029] An embodiment of the present invention provides another technical solution: an electro-absorption modulator laser, comprising a DFB laser and an EAM electro-absorption modulator, wherein deep isolation grooves are provided on both sides of the ridge waveguide or isolation region of the DFB laser, and a window structure is made on the light output end of the EAM electro-absorption modulator.

[0030] Furthermore, the deep isolation trench at least extends to the buffer layer of the laser, and the length of the window structure is controlled between 10 and 50 μm.

[0031] Furthermore, the isolation region is obtained by removing a contact layer and a portion of a P-type waveguide layer between the DFB laser and the EAM electro-absorption modulator.

[0032] Furthermore, the DFB laser is a shallow ridge waveguide structure, the groove depth reaches its grating layer, and the isolation region and the EAM electro-absorption modulator are deep ridge waveguide structures, the groove depth reaches at least their buffer layer.

[0033] Furthermore, the length of the isolation region is controlled to be between 20 and 100 μm.

[0034] Compared with the prior art, the beneficial effects of the present invention are: on the premise that the anti-reflection ability is improved by integrating the light output window of the electro-absorption modulator of the ridge waveguide structure, deep isolation grooves are designed on both sides of the shallow ridge waveguide or isolation area of ​​the DFB laser to greatly reduce the leakage at the docking interface of the docking window during the carrier injection process of the DFB laser, so as to reduce the threshold current of the DFB laser and improve the output optical power of the EML laser. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 A schematic diagram of the structure of an electro-absorption modulator laser after grating embedding provided by an embodiment of the present invention;

[0036] Figure 2 A schematic diagram of the structure of an EAM region of an electro-absorption modulator laser after corrosion provided by an embodiment of the present invention;

[0037] Figure 3 A schematic diagram of the structure of an EAM region active layer of an electro-absorption modulator laser after growth provided by an embodiment of the present invention;

[0038] Figure 4 A schematic diagram of the structure of the light-emitting end of an electro-absorption modulator laser after corrosion provided by an embodiment of the present invention;

[0039] Figure 5 A schematic diagram of the structure of a light-emitting window of an electro-absorption modulator laser provided in an embodiment of the present invention;

[0040] Figure 6 A schematic diagram of the structure of an electro-absorption modulator laser provided by an embodiment of the present invention after the entire surface of the P-type InP waveguide layer and the contact layer are grown;

[0041] Figure 7a A schematic diagram of the structure after the deep isolation trench and isolation region of an electro-absorption modulator laser provided in an embodiment of the present invention are manufactured (embodiment 1);

[0042] Figure 7b for Figure 7a Cross-sectional view of LD region along A direction;

[0043] Figure 7c for Figure 7a A cross-sectional view of the isolation zone along the B direction;

[0044] Figure 7d for Figure 7a Cross-section of the EAM region along the C direction;

[0045] Figure 8a A schematic diagram of the structure after the deep isolation trench and isolation region of an electro-absorption modulator laser provided in an embodiment of the present invention are manufactured (Example 2);

[0046] Figure 8b for Figure 8a Cross-sectional view of LD region along D direction;

[0047] Figure 8c for Figure 8a A cross-sectional view of the isolation zone along the E direction;

[0048] Figure 8d for Figure 8a Cross-section of the EAM region along the F direction;

[0049] Figure 9a A top view of an electrode of an electro-absorption modulator laser provided by an embodiment of the present invention after being manufactured;

[0050] Figure 9b for Figure 9a Cross-sectional view of the EAM region along the G direction. DETAILED DESCRIPTION

[0051] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0052] The embodiment of the present invention provides a method for preparing an electro-absorption modulator laser, which specifically comprises the following steps:

[0053] S1, forming a window structure at the light output end of the EAM region through masking, growth and etching;

[0054] S2, then continue masking and etching to form deep isolation trenches;

[0055] S3, after masking and etching, an electric injection window is opened, wherein the EAM window structure does not have an electric injection window;

[0056] S4, making electrodes in the LD region and the EAM region, wherein the EAM window structure does not serve as an electrode;

[0057] S5, after the electrodes are fabricated, they are decomposed into a single electro-absorption modulator laser chip.

[0058] Since the methods of manufacturing the deep isolation trenches are different, two different embodiments are provided here to explain in detail the specific method of manufacturing the electro-absorption modulator laser.

[0059] Embodiment 1:

[0060] (1) epitaxially growing an InP buffer layer 2, a DFB active layer 3, an InP layer 4, and a grating layer 5 by MOCVD at one time;

[0061] (2) Using holographic or electron beam lithography to make a grating on the LD side grating layer 5, and then using MOCVD secondary epitaxial grating to bury the InP layer 6, see Figure 1 ;

[0062] (3) Growth of SiO 2 The mask layer 7 is used to remove the SiO2 on the EAM side by photolithography and etching technology, and then the EAM side is etched to the InP buffer layer 2 and below by combining dry and wet methods. Figure 2 ;

[0063] (4) SiO 2 The mask layer 7 is used as the mask layer. On the EAM side, the EAM active layer 8 and the InP layer 9 are sequentially grown by MOCVD. Figure 3 , wherein the InP layer 9 is flush with the surface of the InP layer 6;

[0064] (5) Regrowth of SiO 2 The mask layer 7 is used to remove the SiO2 at the EAM side light output end by photolithography and etching technology. The EAM side light output end is etched to the InP buffer layer 2 and below by combining dry etching and wet etching. Figure 4 ;

[0065] (6) SiO 2 The mask layer 7 is used as the mask layer. An InP layer 12 is grown by MOCVD at the light output end of the EAM side to form a window structure, wherein the InP layer 12 is flush with the surface of InP 6. Figure 5 ;

[0066] (7) Remove the mask layer 7 and grow the entire surface P-type InP waveguide layer 10 and contact layer 11. Figure 6 ;

[0067] (8) Growth of SiO 2 For the mask layer, photolithography, dry etching or wet etching are combined to remove the SiO on the EAM window structure. 2 and a contact layer 11;

[0068] (9) Removal of SiO 2 Mask layer, grow SiO again 2 For the mask layer, photolithography, dry etching and wet etching are combined to etch onto the grating layer, and shallow ridge waveguides are made on the LD and EAM sides, wherein no ridge waveguide is made on the light output end of the EA side;

[0069] (10) Protect the LD side with photoresist, and dry or wet etch the isolation area and EAM side ridge waveguide to InP buffer layer 2 and below to make a deep ridge waveguide, see Figure Figure 7a , 7c and 7d;

[0070] (11) Photoresist protects the isolation area, the EAM side and part of the ridge waveguide area, exposing the middle part of the ridge waveguide groove in the LD area. The middle area of ​​the ridge waveguide on the LD side is etched by wet method to the InP buffer layer 2 and below to form a deep isolation groove, as shown in FIG. Figure 7a and 7b ;

[0071] (12) Remove the photoresist and SiO2 mask and re-grow SiO 2 The mask layer 15 is used for photolithography, dry etching and wet etching to remove the SiO2 on the ridge waveguide at the junction of LD and EAM. 2 The mask layer is used to remove the contact layer 11 and part of the P-type InP waveguide layer 10 on the surface of the ridge waveguide in the isolation region. Figure 7c ;

[0072] (13) Photolithography, dry etching or wet etching are combined to remove SiO on the LD and EAM ridge waveguides. 2 A mask is provided to open an electrical injection window, wherein the EAM window structure does not open an electrical injection window;

[0073] (14) Electrodes are fabricated on the LD side and the EAM side, but no electrode is fabricated on the EAM window structure (see FIG9 ).

[0074] (15) After the electrode is made, it is thinned, sputtered, alloyed, and debonded into strips, thin films, and individual chips.

[0075] Embodiment 2:

[0076] (1) epitaxially growing an InP buffer layer 2, a DFB active layer 3, an InP layer 4, and a grating layer 5 by MOCVD at one time;

[0077] (2) Using holographic or electron beam lithography to make a grating on the LD side grating layer 5, and then using MOCVD secondary epitaxial grating to bury the InP layer 6, see Figure 1 ;

[0078] (3) SiO2 is grown as a mask layer 7, and the SiO2 on the EAM side is removed by photolithography and etching techniques. Then, the EAM side is etched to the InP buffer layer 2 and below by combining dry and wet methods. Figure 2 ;

[0079] (4) Using SiO2 as the mask layer 7, the EAM active layer 8 and the InP layer 9 are sequentially grown by MOCVD on the EAM side. Figure 3 , wherein the InP layer 9 is flush with the surface of the InP layer 6;

[0080] (5) Grow SiO2 again as the mask layer 7, and combine photolithography, dry etching and wet etching to etch the light-emitting end of the EAM side to the InP buffer layer 2 and below. Figure 4 ;

[0081] (6) With SiO2 as the mask layer 7, an InP layer 12 is grown by MOCVD at the light-emitting end of the EAM side to form a window structure, wherein the InP layer 12 is flush with the surface of InP 6. Figure 5 ;

[0082] (7) Remove the mask layer 7 and grow the entire surface P-type InP waveguide layer 10 and contact layer 11. Figure 6 ;

[0083] (8) Grow SiO2 as a mask layer, and remove the SiO2 and contact layer 11 on the EAM window structure by combining photolithography, dry etching or wet etching; (then make a deep isolation trench)

[0084] (9) Remove the mask layer 7, grow SiO2 as the mask layer, and use a combination of photolithography, dry etching and wet etching to protect the light output end on the EAM side, make a ridge waveguide on the LD and EAM sides, and at the same time etch away the area outside the ridge waveguide in the isolation area at the junction of the LD and the EAM;

[0085] (10) Protect the LD side with photoresist to expose the isolation area and EAM area. Dry-etch the isolation area and EAM area without mask layer protection area to InP buffer layer 2 and below to form a deep isolation trench in the isolation area. Figure 8a and 8c ;

[0086] (11) Remove the photoresist and SiO2 mask, re-grow SiO2 as the mask layer 15, combine photolithography, dry etching and wet etching to remove the SiO2 mask layer on the isolation region ridge waveguide at the junction of LD and EAM, and then remove the contact layer 11 and part of the P-type InP waveguide layer 10 on the surface of the isolation region ridge waveguide. Figure 8a and Figure 8c ;

[0087] (12) removing the SiO2 mask on the LD and EAM ridge waveguides by combining photolithography, dry etching or wet etching, and opening an electrical injection window, wherein the EAM window structure does not have an electrical injection window;

[0088] (13) Electrodes are fabricated on the LD side and the EAM side, wherein the EAM window structure does not have electrodes, as shown in FIG9 ;

[0089] (14) After the electrode is made, it is thinned, sputtered, alloyed, and debonded into strips, thin films, and individual chips.

[0090] See also Figure 1 To Figure 9, where Figure 1 Schematic diagram of the structure of an electro-absorption modulated laser after grating burial, specifically including an N-type substrate 1, an InP buffer layer 2, a DFB active layer 3, an InP layer 4, a grating layer 5 and a grating-buried InP layer 6. Figure 2 Schematic diagram of the structure of the electro-absorption modulated laser EAM region after etching, specifically including an N-type substrate 1, an InP buffer layer 2, a DFB active layer 3, an InP layer 4, a grating layer 5, a grating buried InP layer 6 and a mask layer 7. Figure 3 Schematic diagram of the structure of the active layer of the EAM region of the electro-absorption modulated laser after growth, specifically including an InP buffer layer 2, a mask layer 7, an EAM active layer 8 and InP 9. Figure 4 Schematic diagram of the structure of the light-emitting end of an electro-absorption modulated laser after corrosion, including a mask layer 7. Figure 5 The schematic diagram of the structure of the light-emitting window of the electro-absorption modulated laser includes a mask layer 7 and a butt-grown InP 12. Figure 6 It is a schematic diagram of the structure of an electro-absorption modulated laser after the entire surface of the P-type InP waveguide layer and the contact layer are grown, including butt-grown InP 12, a P-type InP waveguide layer 10 and a contact layer 11.

[0091] Specifically, an embodiment of the present invention provides an electro-absorption modulator laser, which is composed of a DFB laser and an EAM electro-absorption modulator. A window structure anti-reflection solution is applied at the light output end, and deep isolation grooves are designed on both sides of the DFB laser ridge waveguide or isolation area to reduce leakage, thereby reducing the DFB laser threshold current and improving the output optical power of the EML laser.

[0092] As an optimization solution of the embodiment of the present invention, a window structure is made at the light output end of the EAM electro-absorption modulator to play an anti-reflection role, wherein the length of the window structure is 10 to 50 um and the material is InP.

[0093] As an optimization scheme of an embodiment of the present invention, the DFB laser is a shallow ridge waveguide structure with a groove depth reaching the grating layer, and the isolation region and the EAM electro-absorption modulator are deep ridge waveguide structures with a groove depth reaching the InP buffer layer and below.

[0094] As an optimization solution of the embodiment of the present invention, deep isolation grooves are made on both sides of the DFB laser ridge waveguide or isolation region, wherein the deep isolation grooves extend to the InP buffer layer and below.

[0095] As an optimization scheme of the embodiment of the present invention, after the deep isolation trenches on the LD and EAM sides are completed, an isolation region is made, and the contact layer between the DFB and the EAM and part of the P-type InP waveguide layer are removed to form an isolation region with a length of 20-100 um.

[0096] As an optimization scheme of the embodiment of the present invention, after the isolation area is manufactured, an electric injection window is opened and electrodes are manufactured, wherein the electric injection window of the light output end window structure is not opened and electrodes are not manufactured.

[0097] As an optimization solution of the embodiment of the present invention, after the electrode is manufactured, it is thinned, sputtered, alloyed, and debonded into strips, thin films, and individual chips.

[0098] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing an electroabsorption modulator laser, characterized in that: The prepared electro-absorption modulator laser has an LD region and an EAM region, and specifically includes the following steps: S1, forming a window structure at the light output end of the EAM region through masking, growth and etching; S2, then continue masking and etching to form deep isolation trenches; S3, after masking and etching, an electric injection window is opened, wherein the EAM window structure does not have an electric injection window; S4, making electrodes in the LD region and the EAM region, wherein the EAM window structure does not serve as an electrode; S5, after the electrodes are made, they are decomposed into a single electro-absorption modulator laser chip. In step S1, the specific production process is: S10, growing an epitaxial structure once, and then manufacturing a grating on the epitaxial structure; S11, performing secondary epitaxial growth of a grating buried layer on the grating; S12, then continue to grow the mask layer, remove the mask of the EAM region, and then continue to etch the EAM region, at least etching to the buffer layer of the epitaxial structure; S13, sequentially butt-growing an EAM active layer and an InP layer in the EAM region; S14, growing the mask layer again, and removing the mask at the light-emitting end of the EAM region by etching, and continuing etching until at least the buffer layer is etched; S15, growing an InP layer at the light-emitting end of the EAM region into a window structure; S16, then grow the P-type waveguide layer and contact layer, S17, after the growth is completed, continue to mask and etch away the mask and contact layer on the EAM window structure, The specific method for making deep isolation trenches is: After the mask is formed, etching is performed until the grating layer is etched. Then, shallow ridge waveguides are fabricated in the LD region and the EAM region, wherein no ridge waveguide is fabricated at the light output end of the EAM region. Then, the LD region is protected, and etching is performed in the isolation region and the EAM region, at least to the buffer layer, to produce a deep ridge waveguide, wherein the isolation region is obtained by removing the contact layer and part of the P-type waveguide layer between the DFB laser and the EAM electro-absorption modulator. Protect the isolation region, the EAM region and part of the ridge waveguide region, expose the middle part of the ridge waveguide groove of the LD region, and then continue to etch the middle area of ​​the ridge waveguide of the LD region, at least to the buffer layer, to form a deep isolation groove, or, Etching is performed after masking to protect the light-emitting end of the EAM area, and ridge waveguides are made in the LD area and the EAM area. At the same time, the area outside the ridge waveguide in the isolation area at the junction of the LD area and the EAM area is etched. Next, the LD region is protected to expose the isolation region and the EAM region, and the areas of the isolation region and the EAM region that are not protected by the mask are etched, at least to the buffer layer, to form a deep isolation groove in the isolation region. The isolation region is obtained by removing the contact layer and part of the P-type waveguide layer between the DFB laser and the EAM electro-absorption modulator.

2. The method for preparing an electroabsorption modulator laser according to claim 1, characterized in that: In the step S3, after masking, the mask on the isolation region ridge waveguide at the junction of the LD region and the EAM region is removed by etching, and then the contact layer and the P-type waveguide layer on the surface of the isolation region ridge waveguide are removed.

3. An electro-absorption modulator laser, characterized in that: The method for preparing an electro-absorption modulator laser according to any one of claims 1 or 2 comprises a DFB laser and an EAM electro-absorption modulator, wherein deep isolation grooves are provided on both sides of the ridge waveguide or isolation region of the DFB laser, and a window structure is provided at the light output end of the EAM electro-absorption modulator.

4. The electro-absorption modulator laser according to claim 3, characterized in that: The deep isolation trench at least extends to the buffer layer of the laser, and the length of the window structure is controlled between 10 and 50 μm.

5. The electro-absorption modulator laser according to claim 3, characterized in that: The DFB laser is a shallow ridge waveguide structure, and the groove depth reaches its grating layer. The isolation region and the EAM electro-absorption modulator are deep ridge waveguide structures, and the groove depth reaches at least their buffer layer.

6. The electro-absorption modulator laser of claim 3, wherein: The length of the isolation region is controlled to be 20-100 μm.

Citation Information

Patent Citations

  • Semiconductor quantum well laser and preparation method thereof

    CN113708219A

  • Structure and manufacturing method of electro-absorption modulated laser chip

    CN116111452A

  • Hybrid waveguide structure EML laser and manufacturing method thereof

    CN116706673A

  • Electroabsorption modulated laser

    US20020131466A1

  • Semiconductor optical integrated element

    US20230102522A1