A high thermal conductivity and high activity CoO / MXene catalyst and its preparation method and application

By using high thermal conductivity MXene support to prepare CoO/MXene catalysts, the problems of uneven product distribution and high-temperature exotherm in Fischer-Tropsch synthesis were solved, efficient CO conversion and C6+ selectivity were achieved, and methane selection was reduced and catalyst deactivation phenomena have improved the economic and industrialization level of Fischer-Tropsch technology.

CN117427673BActive Publication Date: 2024-11-22ANHUI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311381991.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-24
Publication Date
2024-11-22
Estimated Expiration
2043-10-24

AI Technical Summary

Technical Problem

In Fischer-Tropsch synthesis, the product distribution follows the ASF distribution, the effective product generation rate is low, and the high-temperature exothermic reaction reduces the catalyst activity and product selectivity.

Method used

The highly thermally conductive active support MXene support was prepared to prepare a high thermally conductive and high-active CoO/MXene catalyst. It dissolves the cobalt salt and additives in the aqueous benzylamine solution, disperse MXene evenly, sonicate and dry, and forms a CoOx-Co composite structure, and is loaded with Li. , Na, K, Zr, Zn elements improve the thermal conductivity and activity of the catalyst.

Benefits of technology

Significantly improve CO conversion rate and C6+ selectivity, reduce methane selectivity, maintain high activity and stability of the catalyst, and do not have obvious inactivation during continuous operation for 1,000 hours, reducing the investment and operation costs of subsequent product separation equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117427673B_ABST
    Figure CN117427673B_ABST
Patent Text Reader

Abstract

The invention discloses a high thermal conductivity and high activity CoO / MXene catalyst and a preparation method and application thereof. The catalyst is made of the following components by weight: 0.1 to 33 parts of CoO, 60 to 90 parts of MXene carriers, and 0.01 to 5 parts of additives. The preparation method comprises the following steps: dissolving a cobalt salt and an additive in an aqueous solution of benzylamine to obtain an active solution; uniformly dispersing the MXene carrier in the active solution, stirring and ultrasonically treating the MXene carrier at room temperature, transferring the MXene carrier to a reaction container, stirring the reaction, filtering, washing, and drying the product to obtain a high thermal conductivity and high activity CoO / MXene catalyst; the catalyst has the characteristics of high thermal conductivity, high activity, high selectivity, and high stability. 6+ The selectivity of the catalyst was over 85%, while the selectivity of the product methane was less than 5%. There was no obvious deactivation of the catalyst selectivity after 1000h of continuous operation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of Fischer-Tropsch synthesis, and in particular to a CoO / MXene catalyst with high thermal conductivity and high activity, and a preparation method and application thereof. Background Art

[0002] The Fischer-Tropsch reaction was first discovered in Germany in 1925 by German chemists Franz Fischer and Hans Tropsch. During World War II, Germany was limited by its oil supply, so the Fischer-Tropsch reaction was widely used in Germany. Fischer-Tropsch synthesis enabled Germany to produce fuel for military and industrial needs during the war. The Fischer-Tropsch reaction was gradually replaced by other energy sources after the war, but it remains an important technology. After entering the 21st century, the world's energy structure has shifted from single oil to coal, oil, natural gas and biomass, and Fischer-Tropsch synthesis technology has further developed rapidly.

[0003] Cobalt-based catalysts have the advantages of high catalytic activity, high chain growth activity and low water vapor shift reaction in Fischer-Tropsch synthesis, and have been widely studied in the field of Fischer-Tropsch synthesis. So far, they have been applied on a large scale in Sasol and Shell. In China, Co-based Fischer-Tropsch synthesis has also gradually entered the industrialization stage.

[0004] According to previous studies, metal Co is traditionally considered to be the active center of the Fischer-Tropsch reaction. Chinese patent document CN201010509275.X discloses a method for preparing a cobalt-based Fischer-Tropsch synthesis catalyst, including a preparation process of a cobalt-based Fischer-Tropsch synthesis catalyst and a hydrothermal treatment process. The preparation process of the cobalt-based Fischer-Tropsch synthesis catalyst uses an impregnation method to load the active component cobalt and an additive onto a catalyst carrier, and the hydrothermal treatment process is to use water vapor for hydrothermal treatment at 150 to 600°C for 0.5 to 20 hours; however, the use of a pure Co-based catalyst will cause the product distribution to follow the ASF (Anderson-Schulz-Flory) distribution, resulting in a low generation rate of specific effective products, making low-cost operation difficult. Moreover, Fischer-Tropsch synthesis is a high-temperature exothermic reaction, and the product is greatly affected by temperature. If the heat accumulated during the Fischer-Tropsch reaction cannot be removed in time, the activity of the catalyst and the selectivity of the product will decrease.

[0005] Therefore, the present invention develops a CoO / MXene catalyst with high thermal conductivity and high activity based on the active carrier MXene with high thermal conductivity. x -Co, this innovative catalyst design is expected to overcome the limitations of traditional Co-based catalysts, improve the yield of specific effective products, and possess excellent catalytic activity and stability. Summary of the invention

[0006] In order to solve the deficiencies of the prior art, the present invention aims to provide a high thermal conductivity and high activity CoO / MXene catalyst and its preparation method and application. The prepared catalyst can significantly improve the conversion rate of CO and C 6+ selectivity and reduce the selectivity of methane.

[0007] In order to achieve the above object, the present invention adopts the following technical solution:

[0008] A high thermal conductivity and high activity CoO / MXene catalyst is prepared from the following components, measured by weight: 0.1 to 33 parts of CoO, 60 to 90 parts of MXene carriers, and 0.01 to 5 parts of additives; the additives are one or more soluble salts of Li, Na, K, Zr, and Zn.

[0009] Preferably, the MXene carrier is one or more of Ti3C2-MXene, Ti2C3-MXene, and Nb2C-MXene.

[0010] Preferably, the specific surface area of ​​the MXene carrier is 10 to 50 m 2 / g, BJH pore size is 5~80nm.

[0011] The present invention also claims a method for preparing the highly thermally conductive and highly active CoO / MXene catalyst, which comprises the following steps:

[0012] (1) dissolving a cobalt salt and an auxiliary agent in an aqueous solution of benzylamine to obtain an active solution;

[0013] (2) The MXene carrier is uniformly dispersed in the active solution, stirred and ultrasonically treated at room temperature, transferred to a reaction vessel, stirred for reaction, and the product is filtered, washed, and dried to obtain a CoO / MXene catalyst with high thermal conductivity and high activity.

[0014] Preferably, in step (1), the cobalt salt is one or more of cobalt acetylacetonate, cobalt nitrate hexahydrate, cobalt chloride or cobalt carbonyl.

[0015] Preferably, in step (1), the cobalt salt is cobalt acetylacetonate and the auxiliary agent is sodium nitrate.

[0016] Preferably, in step (1), the volume ratio of water to benzylamine in the aqueous solution of benzylamine is 20:60-80.

[0017] Preferably, in step (2), the ultrasonic treatment time is 20 to 40 minutes, the reaction conditions are 190 to 220° C. for 1 to 3 hours, and the drying conditions are vacuum drying at 40 to 80° C.

[0018] Preferably, in step (2), the ultrasonic treatment time is 30 min, the reaction conditions are 200° C. for 2 h, and the drying conditions are vacuum drying at 60° C.

[0019] The present invention also claims protection for the use of the highly thermally conductive and highly active CoO / MXene catalyst in the Fischer-Tropsch reaction.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] 1) The present invention provides a high thermal conductivity and high activity CoO / MXene catalyst, which can self-reduced to form CoO by adjusting the additive. x -Co composite structure active components, with high thermal conductivity, high activity, high selectivity, high stability characteristics; under the appropriate catalytic environment, C 6+ The selectivity reaches over 85%, while the selectivity of the product methane is less than 5%. After 1000 hours of continuous operation, there is no obvious deactivation of the catalyst selectivity, which can greatly reduce the equipment investment and operating costs of subsequent product separation, and is conducive to improving the economy of the Fischer-Tropsch technology and its further industrialization.

[0022] 2) The present invention provides a high thermal conductivity and high activity CoO / MXene catalyst, which takes CoO as an active component and is further added with elements such as Li, Na, K, Zr, and Zn, and is loaded on a Mxene carrier; wherein CoO is the active component of the catalyst, and the additive can effectively adjust the crystal size of the Co species and improve the distribution of cobalt on the carrier surface; Mxene is a new type of catalyst active carrier, which has a certain reducibility and has rich active groups on its surface, which can promote the formation of CoOx-Co by the active component on the one hand, and promote the non-dissociative adsorption of CO on the catalyst surface on the other hand, and promote the combination of the surface OH group and the C* formed on the surface of the active component to produce a hydroformylation reaction, thereby improving the activity of the catalyst, promoting the carbon chain growth of the product, and reducing the selectivity of its methane product. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show schematic diagrams of certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 TEM image of the high thermal conductivity and high activity CoO / Mxene catalyst prepared in Example 1 of the present invention;

[0025] Figure 2This is a physical picture of the high thermal conductivity and high activity CoO / Mxene catalyst prepared in Example 1 of the present invention;

[0026] Figure 3 Example 4 of the present invention prepares a high thermal conductivity and high activity CoO / Mxene catalyst and shows the relationship between selectivity and time for 1000 consecutive hours. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical solution and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the embodiments. Of course, the specific embodiments described here are only used to explain the present invention and are not used to limit the present invention.

[0028] Unless otherwise specified, the chemical reagents and materials in the present invention are purchased from commercial sources or synthesized from raw materials purchased from commercial sources.

[0029] The Al2O3 support was purchased from Alfa Aesar with a specific surface area of ​​120 m 2 / g.

[0030] The present invention will be further described below through specific embodiments.

[0031] Example 1

[0032] A method for preparing a high thermal conductivity and high activity CoO / Mxene catalyst comprises the following steps:

[0033] Weigh 1.5 g of cobalt acetylacetonate (C 15 H 21 CoO6) and 0.2g sodium nitrate (NaNO3), and add 40mL of benzylamine and 10mL of ultrapure water, stir to mix well, and obtain an active solution;

[0034] 1.2 g of pre-prepared Ti3C2-MXene was dispersed in the active solution, ultrasonically stirred at room temperature for 30 min, transferred to a three-necked flask with a reflux device on the top, and reacted at 190°C for 2 h under stirring. The product was filtered and washed with ethanol 5 times. The precipitate was collected and dried in a vacuum drying oven at 60°C to obtain a high thermal conductivity and high activity CoO / MXene catalyst recorded as: CoO / MXene-1.

[0035] Example 2

[0036] A method for preparing a high thermal conductivity and high activity CoO / Mxene catalyst comprises the following steps:

[0037] Weigh 1.5 g of cobalt acetylacetonate (C 15 H 21CoO6) and 0.2g sodium nitrate (NaNO3), 0.1g zinc chloride (ZnCl2), and add 40mL benzylamine and 10mL ultrapure water, stir to mix well, and obtain an active solution;

[0038] 1.2 g of pre-prepared Ti3C2-MXene was dispersed in the active solution, ultrasonically stirred at room temperature for 30 min, transferred to a three-necked flask with a reflux device on the top, and kept reacting at 190°C for 2 h under stirring. The product was filtered and washed alternately with ethanol and deionized water for 5 times each. The precipitate was collected and dried in a vacuum drying oven at 60°C to obtain a high thermal conductivity and high activity CoO / MXene catalyst recorded as: CoO / MXene-2.

[0039] Example 3

[0040] A method for preparing a high thermal conductivity and high activity CoO / Mxene catalyst comprises the following steps:

[0041] Weigh 1.5 g of cobalt acetylacetonate (C 15 H 21 CoO6) and 0.2g sodium nitrate (NaNO3), and add 40mL of benzylamine and 10mL of ultrapure water, stir to mix well, and obtain an active solution;

[0042] 1.2 g of pre-prepared Ti2C3-MXene was dispersed in the active solution, ultrasonically stirred at room temperature for 30 min, transferred to a three-necked flask with a reflux device on the top, and reacted at 220°C for 2 h under stirring. The product was filtered and washed with ethanol 5 times. The precipitate was collected and dried in a vacuum drying oven at 60°C to obtain a high thermal conductivity and high activity CoO / MXene catalyst recorded as: CoO / MXene-3.

[0043] Example 4

[0044] A method for preparing a high thermal conductivity and high activity CoO / Mxene catalyst comprises the following steps:

[0045] Weigh 1.22 g of cobalt nitrate (Co(NO3)2·6H2O) and 0.2 g of sodium nitrate (NaNO3), add 40 mL of benzylamine and 10 mL of ultrapure water, stir to mix well, and obtain an active solution;

[0046] 1.2 g of pre-prepared Ti3C2-MXene was dispersed in the active solution, ultrasonically stirred at room temperature for 30 min, transferred to a three-necked flask with a reflux device on the top, and reacted at 220°C for 2 h under stirring. The product was filtered and washed with ethanol 5 times. The precipitate was collected and dried in a vacuum drying oven at 60°C to obtain a high thermal conductivity and high activity CoO / MXene catalyst recorded as: CoO / MXene-4.

[0047] Comparative Example 1

[0048] A method for preparing a CoO / Al2O3 catalyst comprises the following steps:

[0049] Weigh 1.5 g of cobalt acetylacetonate (C 15 H 21 CoO6), and add 40 mL of benzylamine and 10 mL of ultrapure water, stirring to mix well, to obtain an active solution;

[0050] 1.2 g of Al2O3 carrier was dispersed in the active solution, ultrasonically stirred at room temperature for 30 min, transferred to a three-necked flask equipped with a reflux device on the top, and kept reacting at 220°C for 2 h under stirring. The product was filtered and washed with ethanol 5 times. The precipitate was collected and dried in a vacuum drying oven at 60°C to obtain a CoO / Al2O3 catalyst, recorded as: CoO / Al2O3.

[0051] The activity of the catalysts prepared in Examples 1 to 4 and Comparative Example 1 was evaluated. The evaluation test was carried out in a continuously operating fixed bed reactor. 0.25 g of the catalyst was mixed with 0.25 g of quartz sand and then loaded into a stainless steel reaction tube. Asbestos of about 0.5 cm thick was filled above and below the catalyst. The reaction conditions were 240°C, mixed gas flow rate: 20 mL / min, reaction gas pressure: 2.0 MPa, H2 / CO=2 (molar ratio). The evaluation results are shown in Table 1.

[0052] Table 1 FT activity and selectivity of different catalysts

[0053] catalyst CO conversion rate (%) <![CDATA[C 6+ Optional]]> <![CDATA[CH4 selectivity]]> CoO / MXene-1 67.57 85.23 4.05 CoO / MXene-2 70.21 83.11 3.17 CoO / MXene-3 76.32 82.32 3.54 CoO / MXene-4 75.18 83.42 4.63 <![CDATA[CoO / Al2O3]]> 6.93 48.25 27.72

[0054] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. Application of a CoO / MXene catalyst in a Fischer-Tropsch reaction, characterized in that: The CoO / MXene catalyst is made of the following components by weight: 0.1-33 parts of CoO, 60-90 parts of MXene carrier, and 0.01-5 parts of auxiliary agent; the auxiliary agent is one or more soluble salts of Li, Na, K, and Zn; The CoO / MXene catalyst can be self-reduced to form CoO by adjusting the additive. x -The active component of the Co composite structure; The preparation method of the CoO / MXene catalyst comprises the following steps: (1) dissolving the cobalt salt and the auxiliary agent in an aqueous solution of benzylamine to obtain an active solution; (2) The MXene carrier is uniformly dispersed in the active solution, stirred and ultrasonically treated at room temperature, transferred to a reaction vessel, stirred for reaction, and the product is filtered, washed, and dried to obtain a CoO / MXene catalyst.

2. The use according to claim 1, characterized in that: The MXene carrier is one or more of Ti3C2-MXene, Ti2C3-MXene, and Nb2C-MXene.

3. The use according to claim 1, characterized in that: The specific surface area of ​​the MXene carrier is 10~50m 2 / g, BJH pore size is 5~80nm.

4. The use according to claim 1, characterized in that: In step (1), the cobalt salt is one or more of cobalt acetylacetonate, cobalt nitrate hexahydrate, cobalt chloride or cobalt carbonyl.

5. The use according to claim 1, characterized in that: In step (1), the cobalt salt is cobalt acetylacetonate and the auxiliary agent is sodium nitrate.

6. The use according to claim 1, characterized in that: In step (1), the volume ratio of water to benzylamine in the aqueous solution of benzylamine is 20:60-80.

7. The use according to claim 1, characterized in that: In step (2), the ultrasonic treatment time is 20-40 min, the reaction conditions are 190-220° C. for 1-3 h, and the drying conditions are vacuum drying at 40-80° C.

8. The use according to claim 1, characterized in that: In step (2), the ultrasonic treatment time is 30 minutes, the reaction conditions are 200°C for 2 hours, and the drying conditions are vacuum drying at 60°C.