A kind of ceramic fiber fishing net material with antibacterial and durability and preparation method thereof
By using boron nitride reinforced TiO2 ceramic fiber and silver plating in the fishing net material, a "skin-core" structure is formed, which solves the problem of insufficient durability of the fishing net material in the sun, rain and water, and achieves antibacterial properties and durability sexual enhancement.
Patent Information
- Application Number
- CN202311380678.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-24
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-10-24
AI Technical Summary
Existing fishing net materials are prone to aging when exposed to the sun and rain for a long time. Bacteria in the water body are prone to adhere and grow. They have insufficient strength and are easily torn.
Boron nitride (BN) is used to reinforce TiO2 ceramic fiber, and its surface is plated with silver to form a fiber material with a "skin-core" structure. The TiO2 ceramic fiber is infiltrated into B2O3 sol, and then sintered at high temperature and then silver-plated to produce antibacterial properties. and durable ceramic fiber fishing net material.
It improves the antibacterial properties of the fishing net, prevents bacterial growth in the water, and enhances the durability and durability of the fishing net through the oxidation resistance and chemical corrosion resistance of BN.
Smart Images

Figure CN117430414B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic fiber preparation, and in particular relates to a ceramic fiber fishing net material with antibacterial properties and durability and a preparation method thereof. Background Art
[0002] Fishing nets are a tool that is closely related to people's lives. Fishing nets can be used by people for fishing or aquaculture. In ancient times, fishing nets were made of natural fibers (such as hemp, etc.); in modern times, with the rapid development of synthetic material technology, the materials of fishing nets have developed rapidly. The main materials of fishing nets are polyethylene, nylon, etc. These new fishing net materials are widely used. However, polyethylene and nylon have some disadvantages in use, such as: easy aging under long-term sun and rain; various water bacteria are easy to attach to their surface and grow during aquaculture; some fishing nets are not strong enough, so they are easy to be torn, etc. In view of these unfavorable factors, effective solutions are urgently needed to improve the performance of fishing net materials.
[0003] At present, fishing net materials have been widely studied. For example, China Invention Patent Application No. 201610231014.3 discloses a high-strength fishing net. The patent mixes raw materials such as acrylic resin, polyethylene, ethylene-methyl acrylate, and nitrile rubber, and then uses an extruder to granulate, an injection molding machine to inject, and a spinneret to spin, and finally weaves to make a high-strength fishing net; the disadvantage is that the fishing net material of the patent uses many kinds of additives, and the compatibility of these additives needs further discussion. China Invention Patent Application No. 201610008333.8 discloses an ultra-light and high-strength antibacterial and algae-removing fishing net yarn. The patent is made of a blend of polyethylene and nylon, and then an antibacterial and algae-removing coating is coated on the surface of the yarn; the disadvantage of the patent is that the antibacterial and algae-removing coating is easily ineffective after being soaked in water for a long time.
[0004] At present, with the improvement of synthesis technology of new fibers, some new synthetic fibers are widely used in various fields. Among them, ceramic fibers have the advantages of high strength, resistance to sun and rain, and low price. They have broad application space in fishing nets. Literature research shows that there are few research reports in this area. Summary of the invention
[0005] The purpose of the present invention is to provide a ceramic fiber fishing net material with antibacterial properties and durability to solve the shortcomings of the prior art. The surface silver plating of the ceramic fiber fishing net material can improve the antibacterial properties and effectively prevent the growth of water bacteria on the fishing net; its main material boron nitride reinforced TiO2 ceramic fiber has good durability.
[0006] The object of the present invention is to provide a ceramic fiber fishing net material with antibacterial properties and durability. The fishing net material can be prepared by the following preparation method: TiO2 ceramic fiber is infiltrated in B2O3 sol to obtain B2O3-wrapped TiO2 ceramic fiber; then the B2O3-wrapped TiO2 ceramic fiber is sintered at high temperature in an ammonia atmosphere to obtain BN-reinforced TiO2 ceramic fiber; finally, the surface is silver-plated to obtain silver-plated BN-reinforced TiO2 ceramic fiber, that is, the ceramic fiber fishing net material with antibacterial properties and durability.
[0007] Another object of the present invention is to provide a method for preparing the above-mentioned ceramic fiber fishing net material with antibacterial properties and durability, the preparation method comprising the following steps:
[0008] (1) Preparation of TiO2 ceramic fiber: Tetrabutyl titanate is dissolved in anhydrous ethanol to prepare a mixed solution a, 2-hydroxypropionic acid is dissolved in deionized water to prepare a mixed solution b, and the mixed solution b is added dropwise to the mixed solution a, with stirring for 1 to 3 hours, and the reaction temperature is 20°C to 30°C. After the addition is completed, an initial TiO2 sol is obtained; the sol is aged at room temperature for 5 to 8 hours, and the viscosity of the mixed sol is continuously measured, that is, a glass rod is immersed in the sol and slowly lifted up to observe the formation state of thin and long filaments. When the sol meets the viscosity of spinning and its viscosity reaches 25 to 95 Pa•s, the TiO2 sol to be spun is obtained; the sol is spun through a spinning device to obtain fibers; secondly, the fibers are dried at 80°C to 90°C for 5 to 8 hours to obtain gel fibers; then, the gel fibers are sintered at 400°C to 500°C for 3 to 5 hours to obtain TiO2 ceramic fibers.
[0009] Preferably, the volume ratio of tetrabutyl titanate (mL) to anhydrous ethanol (mL) in the mixed solution a is 1:5-10; the volume ratio of 2-hydroxypropionic acid (mL) to deionized water (mL) in the mixed solution b is 1:20-30.
[0010] (2) Preparation of B2O3 sol: Boric acid was dissolved in anhydrous ethanol to prepare a mixed solution a, 10 wt% hydrochloric acid was mixed with anhydrous ethanol to prepare a mixed solution b, and the mixed solution b was added dropwise to the mixed solution a and stirred for reaction. The dropping time was 1 to 2 hours and the reaction temperature was 50°C to 60°C to obtain B2O3 sol.
[0011] Preferably, the mass volume ratio of boric acid (g) to anhydrous ethanol (mL) in the mixed solution a is 1:10-20, and the volume ratio of 10wt% hydrochloric acid (mL) to anhydrous ethanol (mL) in the mixed solution b is 1:20-40.
[0012] (3) Preparation of boron nitride (BN) reinforced TiO2 ceramic fiber: The TiO2 ceramic fiber prepared in step (1) is impregnated with B2O3 sol to obtain B2O3-coated TiO2 ceramic fiber; secondly, the B2O3-coated TiO2 ceramic fiber is dried at 80°C to 90°C for 5 to 7 hours; then, the dried B2O3-coated TiO2 ceramic fiber is sintered at 1100°C to 1200°C in an ammonia atmosphere for 3 to 5 hours to obtain BN-reinforced TiO2 ceramic fiber.
[0013] (4) Surface silver plating of BN-reinforced TiO2 ceramic fiber: Electrochemical silver plating is carried out at room temperature, using a 7-9 mm electrolytic silver rod that has been polished and pickled as the cathode and a 100 mm × 20 mm × 3 mm electrolytic silver plate as the anode, with a distance of 70-80 mm between the two electrodes; the BN-reinforced TiO2 ceramic fiber is placed in the electroplating solution; the surface is mechanically stirred with an electric stirrer, and Ag is deposited and coated at a DC voltage of 5 V for 10 min; the Ag-plated BN-reinforced TiO2 ceramic fiber is washed with distilled water for 3-5 times to obtain a ceramic fiber fishing net material with antibacterial properties and durability.
[0014] Preferably, the electroplating solution comprises 20-40 g / L of AgNO3, 5-10 g / L of KNO3, and 40-50 g / L of C6H5Na3O7•2H2O.
[0015] The present invention has the following notable features:
[0016] (1) The silver-plated BN reinforced TiO2 ceramic fiber prepared by the present invention is a fiber material with a "skin-core" structure, wherein the skin layer is silver-plated BN and the core layer is TiO2; it can meet the requirements of fishing net materials, and its surface silver coating can improve the antibacterial property and effectively prevent the growth of aquatic bacteria on the fishing net; BN has the properties of anti-oxidation and chemical corrosion resistance, and can protect the fishing net from being exposed to the sun, rain or water, thereby improving its durability.
[0017] (2) The inventors of the present application unexpectedly discovered that the B2O3 sol can be wrapped on the surface of TiO2 ceramic fiber by adopting the infiltration method. The "skin layer" of the fiber material with "skin-core" structure prepared by this method can evenly wrap the "core layer".
[0018] (3) The silver-plated BN reinforced TiO2 ceramic fiber prepared by the present invention has a wide range of raw materials, a simple preparation process, and has a good promotion prospect. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 Schematic diagram of the spinning equipment in Examples 1 to 3 (1. spinning solution container; 2. metering pump; 3. gas inlet; 4. filament separation plate; 5. spinning strip; 6. oiling device; 7. godet roller; 8. take-up device);
[0020] Figure 2 Electron microscope image of the TiO2 ceramic fiber in Example 1;
[0021] Figure 3 Schematic diagram of the impregnation equipment in Examples 1 to 3 (9. bracket; 10. yarn collecting plate; 11. impregnation tank; 12. cooling system; 13. traction system; 14. winding bracket). DETAILED DESCRIPTION
[0022] The examples described below illustrate the present invention in detail. Example 1
[0023] In this embodiment, a ceramic fiber fishing net material with antibacterial properties and durability is prepared by the following method, including the following steps:
[0024] (1) Preparation of TiO2 ceramic fiber: 20 mL of tetrabutyl titanate was dissolved in 150 mL of anhydrous ethanol to prepare a mixed solution a, 2 mL of 2-hydroxypropionic acid was dissolved in 50 mL of deionized water to prepare a mixed solution b, and the mixed solution b was added dropwise to the mixed solution a with stirring for 2 hours at a reaction temperature of 25°C. After the addition was completed, an initial TiO2 sol was obtained; the sol was aged at room temperature for 6 hours, and when its viscosity reached 35.7 Pa•s, a TiO2 sol to be spun was obtained; the sol was spun through a spinning device to obtain fibers. The schematic diagram of the spinning device is shown in FIG. Figure 1 As shown; secondly, the fiber was dried at 85°C for 6 hours to obtain gel fiber; then, the gel fiber was sintered at 450°C for 4 hours to obtain TiO2 ceramic fiber. The electron microscope image of the TiO2 ceramic fiber is shown in Figure 2 shown.
[0025] (2) Preparation of B2O3 sol: 5 g of boric acid was dissolved in 75 mL of anhydrous ethanol to prepare a mixed solution a. 5 mL of 10 wt% hydrochloric acid was mixed with 150 mL of anhydrous ethanol to prepare a mixed solution b. The mixed solution b was added dropwise to the mixed solution a and stirred for reaction. The dropping time was 1.5 hours and the reaction temperature was 55°C to obtain B2O3 sol.
[0026] (3) Preparation of BN reinforced TiO2 ceramic fiber: The TiO2 ceramic fiber prepared in step (1) is impregnated with B2O3 sol using an impregnation device such as Figure 3 As shown, B2O3 wrapped TiO2 ceramic fibers were obtained; secondly, the TiO2 ceramic fibers wrapped with B2O3 were dried at 85°C for 6 hours; then, the dried TiO2 ceramic fibers wrapped with B2O3 were sintered at 1150°C in an ammonia atmosphere for 4 hours to obtain BN reinforced TiO2 ceramic fibers.
[0027] (4) Silver plating of BN-reinforced TiO2 ceramic fiber surface: Electrochemical silver plating is carried out at room temperature, using a polished and pickled 8mm electrolytic silver rod as the cathode and a 100mm×20mm×3mm electrolytic silver plate as the anode, with a distance of 75mm between the two electrodes; BN-reinforced TiO2 ceramic fiber is placed in the electroplating solution; mechanically stirred by an electric stirrer, Ag is deposited and coated at a DC voltage of 5V for 10 minutes; Ag-plated BN-reinforced TiO2 ceramic fiber is washed with distilled water for 3 to 5 times to obtain Ag-plated BN-reinforced TiO2 ceramic fiber. The composition of the electroplating solution is 30g / L AgNO3, 7.5g / L KNO3, and 45g / L C6H5Na3O7•2H2O. Example 2
[0028] In this embodiment, a ceramic fiber fishing net material with antibacterial properties and durability is prepared by the following method, including the following steps:
[0029] (1) Preparation of TiO2 ceramic fiber: 20 mL of tetrabutyl titanate was dissolved in 100 mL of anhydrous ethanol to prepare a mixed solution a, 2 mL of 2-hydroxypropionic acid was dissolved in 40 mL of deionized water to prepare a mixed solution b, and the mixed solution b was added dropwise to the mixed solution a with stirring for 1 hour at a reaction temperature of 25°C. After the addition was completed, an initial TiO2 sol was obtained. The sol was aged at room temperature for 6 hours. When the viscosity reached 45.8 Pa•s, a TiO2 sol to be spun was obtained. The sol was spun through a spinning equipment to obtain fibers. Secondly, the fibers were dried at 85°C for 6 hours to obtain gel fibers. Then, the gel fibers were sintered at 400°C for 4 hours to obtain TiO2 ceramic fibers.
[0030] (2) Preparation of B2O3 sol: 5 g of boric acid was dissolved in 50 mL of anhydrous ethanol to prepare a mixed solution a. 5 mL of 10 wt% hydrochloric acid was mixed with 100 mL of anhydrous ethanol to prepare a mixed solution b. The mixed solution b was added dropwise to the mixed solution a and stirred for reaction. The dropping time was 1 hour and the reaction temperature was 50°C to obtain B2O3 sol.
[0031] (3) Preparation of BN reinforced TiO2 ceramic fiber: The TiO2 ceramic fiber prepared in step (1) is impregnated with B2O3 sol using an impregnation device such as Figure 1 As shown, B2O3 wrapped TiO2 ceramic fibers were obtained; secondly, the TiO2 ceramic fibers wrapped with B2O3 were dried at 80°C for 5 hours; then, the dried TiO2 ceramic fibers wrapped with B2O3 were sintered at 1100°C in an ammonia atmosphere for 4 hours to obtain BN reinforced TiO2 ceramic fibers.
[0032] (4) Silver plating of BN-reinforced TiO2 ceramic fiber surface: Electrochemical silver plating is carried out at room temperature, using a 7mm electrolytic silver rod that has been polished and pickled as the cathode, a 100mm×20mm×3mm electrolytic silver plate as the anode, and a distance of 70mm between the two electrodes; the BN-reinforced TiO2 ceramic fiber is placed in the electroplating solution; the Ag is deposited and coated at a DC voltage of 5V using an electric stirrer for 10 minutes; the Ag-plated BN-reinforced TiO2 ceramic fiber is washed with distilled water for 3 times to obtain the Ag-plated BN-reinforced TiO2 ceramic fiber. The composition of the electroplating solution is 20g / L AgNO3, 5g / L KNO3, and 40g / L C6H5Na3O7•2H2O. Example 3
[0033] In this embodiment, a ceramic fiber fishing net material with antibacterial properties and durability is prepared by the following method, including the following steps:
[0034] (1) Preparation of TiO2 ceramic fiber: 20 mL of tetrabutyl titanate was dissolved in 200 mL of anhydrous ethanol to prepare a mixed solution a, 2 mL of 2-hydroxypropionic acid was dissolved in 60 mL of deionized water to prepare a mixed solution b, and the mixed solution b was added dropwise to the mixed solution a with stirring for 3 hours at a reaction temperature of 30°C. After the addition was completed, an initial TiO2 sol was obtained. The sol was aged at room temperature for 6 hours. When the viscosity reached 58.9 Pa•s, a TiO2 sol to be spun was obtained. The sol was spun through a spinning device to obtain fibers. Secondly, the fibers were dried at 85°C for 6 hours to obtain gel fibers. Then, the gel fibers were sintered at 500°C for 4 hours to obtain TiO2 ceramic fibers.
[0035] (2) Preparation of B2O3 sol: 5 g of boric acid was dissolved in 100 mL of anhydrous ethanol to prepare a mixed solution a. 5 mL of 10 wt% hydrochloric acid was mixed with 200 mL of anhydrous ethanol to prepare a mixed solution b. The mixed solution b was added dropwise to the mixed solution a and stirred for reaction. The dropping time was 2 hours and the reaction temperature was 60°C to obtain B2O3 sol.
[0036] (3) Preparation of BN reinforced TiO2 ceramic fiber: The TiO2 ceramic fiber prepared in step (1) is impregnated with B2O3 sol using an impregnation device such as Figure 1 As shown, B2O3 wrapped TiO2 ceramic fibers were obtained; secondly, the TiO2 ceramic fibers wrapped with B2O3 were dried at 90°C for 6 hours; then, the dried TiO2 ceramic fibers wrapped with B2O3 were sintered at 1200°C in an ammonia atmosphere for 4 hours to obtain BN reinforced TiO2 ceramic fibers.
[0037] (4) Silver plating of BN-reinforced TiO2 ceramic fiber surface: Electrochemical silver plating is carried out at room temperature, using a 9mm electrolytic silver rod that has been polished and pickled as the cathode, a 100mm×20mm×3mm electrolytic silver plate as the anode, and a distance of 80mm between the two electrodes; the BN-reinforced TiO2 ceramic fiber is placed in the electroplating solution; an electric stirrer is used to mechanically stir, and Ag is deposited and coated at a DC voltage of 5V for 10 minutes; the Ag-plated BN-reinforced TiO2 ceramic fiber is washed with distilled water for 5 times to obtain the Ag-plated BN-reinforced TiO2 ceramic fiber. The composition of the electroplating solution is 40g / L AgNO3, 10g / L KNO3, and 50g / L C6H5Na3O7•2H2O.
Claims
1. A method for preparing a ceramic fiber fishing net material with antibacterial properties and durability, characterized in that: The preparation method comprises the following steps: (1) Preparation of BN-reinforced TiO2 ceramic fibers: TiO2 ceramic fibers are impregnated with B2O3 sol to obtain B2O3-coated TiO2 ceramic fibers; secondly, the B2O3-coated TiO2 ceramic fibers are dried at 80°C to 90°C for 5 to 7 hours; then, the dried B2O3-coated TiO2 ceramic fibers are sintered at 1100°C to 1200°C in an ammonia atmosphere for 3 to 5 hours to obtain BN-reinforced TiO2 ceramic fibers; (2) Surface silver plating of BN-reinforced TiO2 ceramic fiber: Electrochemical silver plating is carried out at room temperature, using a 7-9 mm electrolytic silver rod that has been polished and pickled as the cathode and a 100 mm × 20 mm × 3 mm electrolytic silver plate as the anode, with a distance of 70-80 mm between the two electrodes; the BN-reinforced TiO2 ceramic fiber is placed in the electroplating solution; the surface is mechanically stirred with an electric stirrer, and Ag is deposited and coated at a DC voltage of 5 V for 10 min; the Ag-plated BN-reinforced TiO2 ceramic fiber is washed with distilled water for 3-5 times to obtain a ceramic fiber fishing net material with antibacterial properties and durability; The preparation method of B2O3 sol in step (1) is as follows: dissolving boric acid in anhydrous ethanol to prepare a mixed solution a, mixing 10% hydrochloric acid with anhydrous ethanol to prepare a mixed solution b, dropping the mixed solution b into the mixed solution a, stirring for reaction, the dropping time is 1 to 2 hours, the reaction temperature is 50°C to 60°C, and the B2O3 sol is obtained.
2. The method for preparing a ceramic fiber fishing net material with antibacterial properties and durability according to claim 1, characterized in that: The preparation method of TiO2 ceramic fiber in the step (1) is as follows: tetrabutyl titanate is dissolved in anhydrous ethanol to obtain a mixed solution c, 2-hydroxypropionic acid is dissolved in deionized water to obtain a mixed solution d, the mixed solution d is added dropwise to the mixed solution c, the stirring and dropping time is 1 to 3 hours, the reaction temperature is 20°C to 30°C, and after the dropping is completed, an initial TiO2 sol is obtained; the sol is aged at room temperature for 5 to 8 hours to obtain a TiO2 sol to be spun; the sol is spun through a spinning device to obtain a fiber; secondly, the fiber is dried at 80°C to 90°C for 5 to 8 hours to obtain a gel fiber; then, the gel fiber is sintered at 400°C to 500°C for 3 to 5 hours to obtain a TiO2 ceramic fiber; the volume ratio of tetrabutyl titanate to anhydrous ethanol in the mixed solution c is: 1 mL: (5 to 10) mL; the volume ratio of 2-hydroxypropionic acid to deionized water in the mixed solution d is: 1 mL: (20 to 30) mL.
3. The method for preparing a ceramic fiber fishing net material with antibacterial properties and durability according to claim 1, characterized in that: The mass volume ratio of boric acid to anhydrous ethanol in the mixed solution a is: 1 g: (10-20) mL, and the volume ratio of 10 wt % hydrochloric acid to anhydrous ethanol in the mixed solution b is: 1 mL: (20-40) mL.
4. The method for preparing a ceramic fiber fishing net material with antibacterial properties and durability according to claim 1, characterized in that: The composition of the electroplating solution in step (2) is 20-40 g / L of AgNO3, 5-10 g / L of KNO3, and 40-50 g / L of C6H5Na3O7•2H2O.
5. A ceramic fiber fishing net material with antibacterial properties and durability, characterized in that: The ceramic fiber fishing net material is prepared by the method for preparing a ceramic fiber fishing net material with antibacterial properties and durability as described in any one of claims 1 to 4.