Preparation method of antibacterial high-water-absorption baby paper diaper
By combining modified PET fibers and antibacterial components, the problem of insufficient antibacterial performance of existing infant diapers is solved, and strong water absorption and long-term antibacterial effects are achieved, which improves the nursing performance of infant diapers.
Patent Information
- Application Number
- CN202411309688.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing baby diapers ignore infant skin sensitivity and antibacterial properties in the process of improving fluid absorption, resulting in an increased risk of diaper rash and bacterial infection.
Modified PET fiber is used as the skin-friendly layer, and hot melt adhesive bonding and double-light roller compaction are performed by adding antibacterial and strong water-absorbing baby diapers. Combined with hot pressing composite technology, the fiber is enhanced. Mechanical strength and antibacterial properties.
It achieves rapid absorption of urine, reduces the contact time between urine and skin, and has a long-term antibacterial effect, avoids the problems of antibacterial agent volatility and fiber strength, and provides a safer nursing environment.
Smart Images

Figure CN119083036A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of daily necessities, and in particular to a method for preparing an antibacterial and highly absorbent baby diaper. Background Art
[0002] During the growth of babies, diapers, as a necessity for daily care, play a vital role. It not only provides great convenience for caregivers, but also protects the healthy growth of babies. Baby diapers are mainly composed of three parts: surface coating layer, absorbent core layer and base fabric. The surface coating layer is close to the baby's skin, can quickly penetrate urine and effectively prevent back-seepage, keeping the surface dry. The absorbent core layer is the core of the diaper, composed of materials such as fluff pulp and super absorbent resin, responsible for absorbing and storing urine, and the base fabric plays a role in leak prevention. Since the surface coating layer is in direct contact with the skin, its material and functionality have a decisive influence on the effectiveness of diapers.
[0003] Since baby skin is delicate and sensitive, especially to humid environment, and humid environment is easy to breed bacteria, which is very unfavorable for baby's growth. Therefore, the skin-friendly layer of baby diapers should have good water absorption, quickly absorb and lock urine, reduce the time of urine contact with skin, and thus reduce the risk of diaper rash. At the same time, it should also have good antibacterial properties to reduce the possibility of bacterial infection and provide a favorable environment for baby's growth.
[0004] Existing diapers often focus on improving the absorbent core layer, but this approach ignores the problem of high sensitivity of baby skin. Although it can make the diapers have excellent liquid absorption effect, the antibacterial performance cannot be guaranteed, which is not conducive to skin care. Summary of the invention
[0005] In order to solve the problems mentioned in the background technology, the object of the present invention is to provide a method for preparing antibacterial and highly absorbent baby diapers.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A method for preparing antibacterial and highly absorbent baby diapers comprises the following steps:
[0008] The first step is to weave the modified PET fiber into a non-woven fabric by adopting a textile process to form a skin-friendly layer;
[0009] The second step is to mix the super absorbent resin, polyvinyl alcohol fiber and fluff pulp to form a mixture, and then shape it in a mold, and then wrap it with wet-strength paper after demolding, and then bond it with hot melt adhesive at a temperature of 120-125°C, and finally compact it with double smooth rollers at a temperature of 110-115°C, cut it, and form an absorption layer;
[0010] The third step is to use polyacrylonitrile fiber as raw material and weave it into non-woven fabric through a weaving process to obtain a barrier layer;
[0011] In the fourth step, the skin-friendly layer in the first step, the absorption layer in the second step and the barrier layer in the third step are stacked and hot-pressed to obtain the antibacterial and highly absorbent baby diapers.
[0012] As a further embodiment of the present invention, in the first step, the method for preparing the modified PET fiber comprises the following steps:
[0013] Step 1: According to the weight ratio, 30-45 parts of PET masterbatch, 2-3.5 parts of antibacterial component, 3-5 parts of water absorbing functional component and 0.5-1.5 parts of antioxidant are mixed evenly, and then fed into a twin-screw extruder for melt extrusion, and then subjected to a pelletizing process to form pellets;
[0014] Step 2: Using a melt spinning process, the pellets in step 1 are melt-spinned to obtain modified PET fibers.
[0015] As a further embodiment of the present invention, in step 1, the method for preparing the antibacterial component comprises the following steps:
[0016] Lignin and N,N-dimethylformamide are mixed and mechanically stirred to form a uniform liquid, then an anhydride bridging agent is added to the liquid. After the addition is completed, it is stirred at room temperature for 2-4 hours, and then citronellol and a catalyst are added to the liquid. The temperature is gradually increased to 90-100°C. After heat preservation for 6-9 hours, the solvent is evaporated, the temperature is reduced and the material is discharged to obtain the antibacterial component.
[0017] As a further embodiment of the present invention, in step 1, the anhydride bridging agent is any one of maleic anhydride, succinic anhydride or glutaric anhydride.
[0018] As a further embodiment of the present invention, in step 1, the catalyst is p-toluenesulfonic acid.
[0019] In the above technical scheme, lignin is modified by using an anhydride bridging agent, and the esterification ring-opening reaction between the hydroxyl groups in the lignin structure and the anhydride bridging agent is utilized to achieve carboxyl modification of the lignin, thereby obtaining a lignin intermediate containing a carboxyl substituent, and then further undergoing esterification condensation with the hydroxyl groups in the citronellol structure under the action of a catalyst, thereby introducing the natural antibacterial agent citronellol into the lignin structure to obtain an antibacterial component.
[0020] As a further embodiment of the present invention, the preparation method of the water absorbing functional component comprises the following steps:
[0021] Step A, add diethylene glycol dichloroethyl ester and toluene to a reactor filled with nitrogen, start stirring, and after forming a uniform mixed liquid, add 2,3-dihydroxypropane-1-sulfonic acid to the reactor, and add sodium hydroxide solution. After the addition is complete, increase the temperature to 70-80° C., keep stirring for 6-9 hours, cool and discharge the material to obtain a cross-linked body;
[0022] Step B: add sodium alginate to purified water, stir evenly, then add activator and condensing agent, stir at room temperature for 1-2 hours, then add cross-linker, after adding, continue mechanical stirring at room temperature for 8-12 hours, then pour the material into a mold, after it forms a gel, place it in a freeze dryer, freeze-thaw cycle 2-4 times, take it out, crush it, and the water-absorbing functional component can be obtained.
[0023] As a further embodiment of the present invention, in step A, the molar ratio of diethylene glycol dichloroethyl ester to 2,3-dihydroxypropane-1-sulfonic acid is 1:1-1.2.
[0024] As a further solution of the present invention, in step A, the mass fraction of the sodium hydroxide solution is 20-30%.
[0025] As a further embodiment of the present invention, in step B, the activating agent is dicyclohexylcarbodiimide or 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride.
[0026] As a further embodiment of the present invention, in step B, the condensing agent is 4-dimethylaminopyridine or N-hydroxysuccinimide.
[0027] In the above technical scheme, diethylene glycol dichloroethyl ester and 2,3-dihydroxypropane-1-sulfonic acid are first used as raw materials, and under the catalytic action of sodium hydroxide, continuous substitution reactions can be carried out between them to obtain a macromolecular compound connected by ether bonds. By controlling the molar ratio of the two, the macromolecular compound is made to be hydroxyl-terminated to obtain a cross-linked body, and then an activator and a condensation agent are used to activate sodium alginate, and then cross-linking polymerization is carried out with the cross-linked body to form a sodium alginate polymer, and then a sodium alginate-based aerogel material, that is, a water-absorbing functional component, can be obtained through a freeze-drying process.
[0028] Beneficial effects of the present invention:
[0029] (1) The present invention starts with the skin-friendly layer material, uses PET as the main raw material, and adds antibacterial components for antibacterial modification. The lignin in the antibacterial component structure has a plasticizing effect, which can improve the mechanical strength of the PET fiber. The natural antibacterial agent citronellol contained in its structure has a broad-spectrum antibacterial effect, which can prevent the growth and reproduction of bacteria. In addition, after the small molecule antibacterial agent citronellol is grafted into the lignin structure, its volatilization and migration phenomenon can be avoided, thereby ensuring the long-term antibacterial performance of the PET fiber and avoiding the problem of the antibacterial agent volatilizing during the storage of the diaper and losing the antibacterial effect.
[0030] (2) The present invention prepares a sodium alginate-based aerogel material by preparing a macromolecular compound connected by an ether bond as a cross-linking agent, and uses the alginate-based aerogel material as a water-absorbing functional component to perform blending and spinning with PET fibers. On the one hand, the aerogel material contains a large number of pore structures and can accommodate a large amount of water. On the other hand, since the cross-linked structure contains a large number of hydrophilic ether bonds and sulfonic acid groups, the aerogel material can exhibit extremely strong hydrophilicity, thereby being able to achieve rapid absorption and storage of urine, allowing the skin to be in a dry environment for a long time. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0032] Figure 1 This is a scanning electron microscope image of the water-absorbing functional component. DETAILED DESCRIPTION
[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Preparation Example 1
[0035] Preparation of antimicrobial components:
[0036] 1.5 g of lignin and N,N-dimethylformamide were mixed and mechanically stirred to form a uniform liquid. Then, 0.2 g of succinic anhydride was added to the liquid. After the addition, it was stirred at room temperature for 3 hours. Then, 0.3 g of citronellol and 0.01 g of p-toluenesulfonic acid were added to the liquid. The temperature was gradually increased to 95°C. After heat preservation for 8 hours, the solvent was evaporated, the temperature was lowered and the material was discharged to obtain the antibacterial component.
[0037] The breakfast titration test method was used to test the ester content in the antibacterial component structure. The test results showed that the ester content was 1.507 mmol / g, indicating that citronellol and lignin were connected by ester bonds.
[0038] Preparation Example 2
[0039] Preparation of water absorbing functional components:
[0040] Step A, add 0.8g of diethylene glycol dichloroethyl ester and toluene to a reactor filled with nitrogen, start stirring, and after forming a uniform mixed liquid, add 0.6g of 2,3-dihydroxypropane-1-sulfonic acid to the reactor, and add 15mL of a 30% sodium hydroxide solution by mass. After the addition is complete, raise the temperature to 75°C, keep stirring for 9h, cool and discharge the material to obtain a cross-linked body;
[0041] Step B, add 1.8g of sodium alginate to purified water, stir well, then add 0.2g of dicyclohexylcarbodiimide and 0.06g of 4-dimethylaminopyridine, stir at room temperature for 2h, then add 0.4g of cross-linked body, after adding, continue to mechanically stir at room temperature for 9h, then pour the material into a mold, after it forms a gel, place it in a freeze dryer, freeze-thaw cycle 3 times, take it out, and crush it to obtain the water-absorbing functional component.
[0042] Figure 1 This is a scanning electron microscope image of the water-absorbing functional component. It can be observed that it has a rich pore structure and the pores are uniform, which can absorb and hold a large amount of water and improve the water absorption of the fiber.
[0043] Example 1
[0044] Preparation of modified PET fiber:
[0045] Step 1: According to the weight ratio, 30 parts of PET masterbatch, 2 parts of antibacterial component, 3 parts of water absorption functional component and 0.5 parts of antioxidant 1010 are mixed evenly, and then fed into a twin-screw extruder for melt extrusion, and the temperature of each zone is controlled to be 240°C, 250°C, 260°C, 260°C and 250°C in sequence, and then subjected to a pelletizing process to form pellets;
[0046] Step 2: Transfer the pellets from step 1 to a melt spinning machine, compact them with a press rod, control the temperature to 230° C., perform melt spinning at a spinning speed of 150 m / min, and then undergo a winding process to obtain modified PET fibers.
[0047] The preparation method of the above antibacterial component is shown in Preparation Example 1; the preparation method of the water absorbing functional component is shown in Preparation Example 2, and the following are the same.
[0048] Example 2
[0049] Preparation of modified PET fiber:
[0050] Step 1: According to the weight proportions, 40 parts of PET masterbatch, 3 parts of antibacterial components, 4.5 parts of water-absorbing functional components, and 1 part of antioxidant 1010 are mixed evenly, and then fed into a twin-screw extruder for melt extrusion, and the temperature of each zone is controlled to be 240° C., 250° C., 260° C., 260° C., and 250° C. in sequence, and then subjected to a pelletizing process to form pellets;
[0051] Step 2: Transfer the pellets from step 1 to a melt spinning machine, compact them with a press rod, control the temperature to 230° C., perform melt spinning at a spinning speed of 150 m / min, and then undergo a winding process to obtain modified PET fibers.
[0052] Example 3
[0053] Preparation of modified PET fiber:
[0054] Step 1: According to the weight proportions, 45 parts of PET masterbatch, 3.5 parts of antibacterial component, 5 parts of water absorbing functional component and 1.5 parts of antioxidant 1010 are mixed evenly, and then fed into a twin-screw extruder for melt extrusion, and the temperature of each zone is controlled to be 240°C, 250°C, 260°C, 260°C and 250°C in sequence, and then subjected to a pelletizing process to form pellets;
[0055] Step 2: Transfer the pellets from step 1 to a melt spinning machine, compact them with a press rod, control the temperature to 230° C., perform melt spinning at a spinning speed of 150 m / min, and then undergo a winding process to obtain modified PET fibers.
[0056] Comparative Example 1
[0057] Preparation of modified PET fiber:
[0058] Step 1: According to the weight ratio, 40 parts of PET masterbatch, 3 parts of citronellol, 4.5 parts of water-absorbing functional components and 1 part of antioxidant 1010 are mixed evenly, and then fed into a twin-screw extruder for melt extrusion, and the temperature of each zone is controlled to be 240° C., 250° C., 260° C., 260° C. and 250° C. in sequence, and then subjected to a pelletizing process to form pellets;
[0059] Step 2: Transfer the pellets from step 1 to a melt spinning machine, compact them with a press rod, control the temperature to 230° C., perform melt spinning at a spinning speed of 150 m / min, and then undergo a winding process to obtain modified PET fibers.
[0060] Comparative Example 2
[0061] Preparation of modified PET fiber:
[0062] Step 1: According to the weight ratio, 40 parts of PET masterbatch, 4.5 parts of water-absorbing functional components and 1 part of antioxidant 1010 are mixed evenly, and then fed into a twin-screw extruder for melt extrusion, and the temperature of each zone is controlled to be 240°C, 250°C, 260°C, 260°C and 250°C in sequence, and then pelletized to form pellets;
[0063] Step 2: Transfer the pellets from step 1 to a melt spinning machine, compact them with a press rod, control the temperature to 230° C., perform melt spinning at a spinning speed of 150 m / min, and then undergo a winding process to obtain modified PET fibers.
[0064] Comparative Example 3
[0065] Preparation of modified PET fiber:
[0066] Step 1: According to the weight percentage, 40 parts of PET masterbatch, 3 parts of antibacterial components and 1 part of antioxidant 1010 are mixed evenly, and then fed into a twin-screw extruder for melt extrusion, and the temperature of each zone is controlled to be 240°C, 250°C, 260°C, 260°C and 250°C in sequence, and then pelletized to form pellets;
[0067] Step 2: Transfer the pellets from step 1 to a melt spinning machine, compact them with a press rod, control the temperature to 230° C., perform melt spinning at a spinning speed of 150 m / min, and then undergo a winding process to obtain modified PET fibers.
[0068] Test Case
[0069] a. According to standard GB / T 14344-2008, the modified PET fibers in Examples 1 to 3 and Comparative Examples 1 to 3 were tested for mechanical strength;
[0070] b. Using a plain weaving process, the modified PET fibers in Example 1, Example 1 to Example 3 and Comparative Example 1 to Comparative Example 3 were made into sample cloths with a specification of 10 cm×10 cm, and the water absorption rate was tested according to the standard GB / T 1655.1-2008;
[0071] c. Each modified PET fiber was made into a 5 cm × 5 cm sample cloth, and placed in an environment of 25°C and 50% relative humidity for 2 months. Then, the antibacterial rate test was performed according to the standard GB / T 20944.3-2008, and the test bacteria was Staphylococcus aureus;
[0072] The test results are recorded in Table 1:
[0073] Table 1 - Test results
[0074] Breaking strength (cN / dtex) Water absorption (%) Antibacterial rate (%) Example 1 4.1 398.4 99.1 Example 2 4.2 401.5 99.2 Example 3 3.9 401.2 99.1 Comparative Example 1 3.1 395.1 81.4 Comparative Example 2 3.0 393.8 51.9 Comparative Example 3 3.8 287.6 99.0
[0075] The analysis and test results show that the modified PET fiber prepared by using antibacterial components and water-absorbing functional components as additives has high mechanical strength, excellent water absorption rate and antibacterial properties. The fiber prepared by directly using citronellol as an antibacterial agent undergoes volatilization migration after being placed for 2 months, which greatly weakens the antibacterial properties of the fiber, and loses the plasticizing effect of lignin, resulting in a decrease in the strength of the fiber. After the antibacterial component is completely removed, the antibacterial properties of the fiber are greatly reduced. After the water-absorbing functional component is removed, the water absorption rate of the fiber is also greatly reduced.
[0076] Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core ideas, including the best mode, and also enable any technician in the field to practice the present invention, including making and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements similar to the literal expression of the claims, or if they include equivalent structural elements that are not substantially different from the literal expression of the claims, then these other embodiments should also be included in the scope of the claims.
[0077] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing antibacterial and highly absorbent baby diapers, It is characterized in that The following steps are involved: The first step is to weave the modified PET fiber into a non-woven fabric by adopting a textile process to form a skin-friendly layer; The second step is to mix the super absorbent resin, polyvinyl alcohol fiber and fluff pulp to form a mixture, and then shape it in a mold, and then wrap it with wet-strength paper after demolding, and then bond it with hot melt adhesive at a temperature of 120-125°C, and finally compact it with double smooth rollers at a temperature of 110-115°C, cut it, and form an absorption layer; The third step is to use polyacrylonitrile fiber as raw material and weave it into non-woven fabric through a weaving process to obtain a barrier layer; In the fourth step, the skin-friendly layer in the first step, the absorption layer in the second step and the barrier layer in the third step are stacked and hot-pressed to obtain the antibacterial and highly absorbent baby diapers.
2. A method for preparing an antibacterial and highly absorbent baby diaper according to claim 1, It is characterized in that In the first step, the preparation method of the modified PET fiber comprises the following steps: Step 1: According to the weight ratio, 30-45 parts of PET masterbatch, 2-3.5 parts of antibacterial component, 3-5 parts of water absorbing functional component and 0.5-1.5 parts of antioxidant are mixed evenly, and then fed into a twin-screw extruder for melt extrusion, and then subjected to a pelletizing process to form pellets; Step 2: Using a melt spinning process, the pellets in step 1 are melt-spinned to obtain modified PET fibers.
3. A method for preparing an antibacterial and highly absorbent baby diaper according to claim 2, It is characterized in that In step 1, the preparation method of the antibacterial component comprises the following steps: Lignin and N,N-dimethylformamide are mixed and mechanically stirred to form a uniform liquid, then an anhydride bridging agent is added to the liquid. After the addition is completed, it is stirred at room temperature for 2-4 hours, and then citronellol and a catalyst are added to the liquid. The temperature is gradually increased to 90-100°C. After heat preservation for 6-9 hours, the solvent is evaporated, the temperature is reduced and the material is discharged to obtain the antibacterial component.
4. A method for preparing an antibacterial and highly absorbent baby diaper according to claim 3, It is characterized in that In step 1, the anhydride bridging agent is any one of maleic anhydride, succinic anhydride or glutaric anhydride.
5. The method for preparing the antibacterial and highly absorbent baby diaper according to claim 3, It is characterized in that In step 1, the catalyst is p-toluenesulfonic acid.
6. A method for preparing an antibacterial and highly absorbent baby diaper according to claim 2, It is characterized in that The preparation method of the water absorbing functional component comprises the following steps: Step A, add diethylene glycol dichloroethyl ester and toluene to a reactor filled with nitrogen, start stirring, and after forming a uniform mixed liquid, add 2,3-dihydroxypropane-1-sulfonic acid to the reactor, and add sodium hydroxide solution. After the addition is complete, increase the temperature to 70-80° C., keep stirring for 6-9 hours, cool and discharge the material to obtain a cross-linked body; Step B: add sodium alginate to purified water, stir evenly, then add activator and condensing agent, stir at room temperature for 1-2 hours, then add cross-linker, after adding, continue mechanical stirring at room temperature for 8-12 hours, then pour the material into a mold, after it forms a gel, place it in a freeze dryer, freeze-thaw cycle 2-4 times, take it out, crush it, and the water-absorbing functional component can be obtained.
7. A method for preparing an antibacterial and highly absorbent baby diaper according to claim 6, It is characterized in that In step A, the molar ratio of diethylene glycol dichloroethyl ester to 2,3-dihydroxypropane-1-sulfonic acid is 1:1-1.
2.
8. The method for preparing the antibacterial and highly absorbent baby diaper according to claim 6, It is characterized in that In step A, the mass fraction of the sodium hydroxide solution is 20-30%.
9. The method for preparing the antibacterial and highly absorbent baby diaper according to claim 6, It is characterized in that In step B, the activating agent is dicyclohexylcarbodiimide or 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride.
10. The method for preparing the antibacterial and highly absorbent baby diaper according to claim 6, It is characterized in that In step B, the condensation agent is 4-dimethylaminopyridine or N-hydroxysuccinimide.
Citation Information
Cited By
High-water-absorption fiber for paper diaper and preparation method of high-water-absorption fiber
CN120060995A
High water-absorbing fiber for paper diaper and method for preparing the same
CN120060995B