Energy-saving coke oven door bricks with enhanced thermal insulation and corrosion resistance and preparation method thereof
Through the mixing of silica particles of multiple particle sizes and the combination of calcium alginate and nano-silicon dioxide, a fine pore structure is formed, which solves the problems of poor insulation performance and insufficient corrosion resistance of coke oven tile bricks, and achieves efficient heat retention and Corrosion resistance.
Patent Information
- Application Number
- CN202311464913.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-07
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-11-07
AI Technical Summary
The insulation performance of existing coke oven door bricks is poor, resulting in slow heating speed of the coke oven combustion chamber, serious heat loss, and insufficient corrosion resistance.
Mixed silica particles of multiple particle sizes, combined with sulfite paper waste slurry as a binding agent, sodium alginate and calcium chloride form calcium alginate, and combined with nano-silica, promoting the transformation of quartz crystals through hot and cold cycles to form Fine pore structure to improve thermal insulation and corrosion resistance.
It significantly improves the insulation and corrosion resistance of the coke oven door bricks, enhances its strength and high temperature resistance, and reduces the thermal conductivity and mass loss.
Smart Images

Figure BDA0004533297290000101 
Figure BDA0004533297290000111 
Figure BDA0004533297290000131
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of refractory materials, and in particular to energy-saving coke oven door bricks with enhanced thermal insulation and corrosion resistance and a preparation method thereof. Background Art
[0002] Coke oven is a thermal equipment with long service life, complex structure and continuous production. It heats coal to 950℃~1100℃ and then distills it to produce coke and chemical products. It is mainly composed of carbonization chamber, combustion chamber, furnace top, ramp, heat storage chamber and small flue. The main function of the coke oven door is to close the carbonization chamber to make it a sealed space for coking. When designing the lining bricks of the coke oven door, both the thermal insulation performance and the structural strength of the lining bricks should be considered.
[0003] Silica bricks have stable high-temperature performance, high load softening temperature close to refractoriness, high thermal conductivity, low high-temperature creep rate, and excellent corrosion resistance. They are ideal high-temperature resistant materials. Therefore, silica bricks are widely used in the vaults of coke ovens, hot blast stoves, glass kilns, tunnel kilns, and shelf bricks of various kilns. However, silica bricks have poor thermal insulation performance. If silica bricks are used as coke oven door bricks, the temperature rise rate of the coke oven combustion chamber will be slow and the heat loss will be serious. Therefore, an energy-saving coke oven door brick with enhanced thermal insulation and corrosion resistance is proposed. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides energy-saving coke oven door bricks with enhanced thermal insulation and corrosion resistance and a preparation method thereof.
[0005] The technical solution of the present invention is: an energy-saving coke oven door brick with enhanced thermal insulation and corrosion resistance, wherein the raw materials of the door brick include, by weight: 70 to 85 parts of silica, 1 to 5 parts of composite mineralizer, 3 to 8 parts of binder, and 2 to 6 parts of additive;
[0006] The silica comprises, by mass percentage, 50-70% silica aggregate, 10-20% silica coarse powder, and the rest silica fine powder, wherein the particle size of the silica aggregate is 1-4.5 mm, the particle size of the silica coarse powder is 340-500 μm, and the particle size of the silica fine powder is 5-20 μm;
[0007] The composite mineralizer comprises, by weight, 0.35 to 1.60 parts of fluorite powder, 0.03 to 0.35 parts of iron phosphorus, 0.55 to 1.90 parts of calcium chloride, 0.04 to 0.80 parts of sodium alginate, and 0.03 to 0.35 parts of nano silicon dioxide.
[0008] Description: The furnace door bricks with the above ingredients are mixed with silica particles of various sizes to make the internal structure of the furnace door bricks uniform, promote the transformation of the internal quartz crystals through the mineralizer, and generate fine and uniform pores inside the brick body, so that the final furnace door bricks have good thermal insulation performance, high strength and excellent corrosion resistance.
[0009] Furthermore, the binder is sulfite paper waste slurry with a specific gravity of 1.18 to 1.28 g / ml.
[0010] Description: The above binder can effectively improve the strength and hardness of furnace door bricks, and improve the high temperature resistance of furnace door bricks.
[0011] Furthermore, the additive is a mixture of any one or more of silicon carbide or silicon nitride in any ratio.
[0012] Description: The additives of the above ingredients have good high-temperature performance, can promote the sintering of furnace door bricks, and improve the density of furnace door bricks.
[0013] Furthermore, the preparation method of the composite mineralizer is:
[0014] S1: adding nano-silicon dioxide to deionized water, and ultrasonically dispersing for 5 to 8 minutes to obtain a nano-silicon dioxide dispersion with a mass concentration of 5 to 8%;
[0015] S2: adding sodium alginate to deionized water to prepare a sodium alginate gel solution with a mass concentration of 5%, and then diluting the sodium alginate gel solution by 10 to 20 times to obtain a sodium alginate diluted solution;
[0016] S3: using a planetary ball mill to uniformly mix fluorite powder, iron phosphorus and calcium chloride to obtain a mixed powder;
[0017] S4: stirring the sodium alginate dilution liquid, and subjecting the sodium alginate dilution liquid to a hot and cold cycle between a high temperature and a low temperature, wherein the high temperature is 30-40° C. and the low temperature is 0-6° C. During the hot and cold cycle, when the temperature of the sodium alginate dilution liquid rises to a high temperature, a nano-silicon dioxide dispersion liquid is added to the sodium alginate dilution liquid once, and when the temperature of the sodium alginate dilution liquid drops to 10-15° C., a mixed powder is added to the sodium alginate dilution liquid once; the single addition amount of the nano-silicon dioxide dispersion liquid accounts for 15-25% of the total amount thereof; the single addition amount of the mixed powder accounts for 20-30% of its weight, until the nano-silicon dioxide dispersion liquid and the mixed powder are all added to the sodium alginate dilution liquid to obtain a mixed liquid;
[0018] S5: filtering, crushing and drying the solid particles in the mixed solution in sequence to obtain a composite mineralizer.
[0019] Description: The above-mentioned composite mineralizer generates calcium alginate through sodium alginate and calcium chloride. Calcium alginate will combine with nano-silicon dioxide to become silica hybrid calcium alginate, and promote the formation of calcium alginate through hot and cold cycles. The silica hybrid calcium alginate and other ingredients work together to promote the conversion of quartz crystals to tridymite during sintering, reduce the residual quartz content, and make the furnace door bricks have fine and uniform pores inside after sintering, thereby improving the thermal insulation performance of the furnace door bricks.
[0020] Furthermore, in step S3, the ball-to-material ratio of the planetary ball mill is 1 to 3:1, and the ball milling time is 10 to 25 minutes.
[0021] Note: Limiting the ball-to-material ratio and ball milling time can ensure that fluorite powder, iron phosphorus and calcium chloride are evenly mixed.
[0022] Furthermore, in step S4, the temperature change rate during the hot and cold cycle is 3-6°C / min.
[0023] Note: Limiting the temperature change rate during hot and cold cycles can ensure the stability of the reaction between sodium alginate and calcium chloride, allowing sodium alginate to react fully.
[0024] Furthermore, in step S5, the solid particles are crushed to a particle size of ≤125 μm.
[0025] Note: Limiting the particle size of the solid particles after crushing can ensure that the mineralizer can be evenly mixed with other raw materials and the stress in the furnace door bricks is concentrated.
[0026] On the other hand, the present invention provides a method for preparing the above-mentioned furnace door brick, comprising the following steps:
[0027] Step 1: Add silica aggregate, silica coarse powder and silica fine powder to a wet mill in sequence, dry mix for 3 to 5 minutes, add additives and composite mineralizers to the wet mill, then add a binder and mix for 10 to 15 minutes, and obtain mud after mixing;
[0028] Step 2: using a press to press the mud into a brick, and then drying the brick at 220-240° C. for 20-22 hours to obtain a dried brick;
[0029] Step 3: Place the dried bricks into a tunnel kiln and heat them to 1380-1480°C for firing. The firing time is 82-85 hours. After firing, furnace door bricks are obtained.
[0030] Description: The furnace door bricks prepared by the above preparation method have uniform structure, fewer internal defects, high yield rate, and good high temperature resistance and corrosion resistance.
[0031] Furthermore, in step 3, the heating process is: firstly, the temperature is increased to 700-750°C at a heating rate of 20-25°C / h, then increased to 1000-1100°C at a heating rate of 15-20°C / h, then increased to 1250-1300°C at a heating rate of 5-10°C / h, kept warm for 1-2h, and then increased to 1380-1480°C at a heating rate of 2-5°C / h.
[0032] Note: The above heating method can ensure the heating speed, improve production efficiency, and avoid cracks in the furnace door bricks due to excessive internal volume expansion during firing.
[0033] The beneficial effects of the present invention are:
[0034] (1) The furnace door brick of the present invention is made of a mixture of silica particles of various particle sizes to make the internal structure of the furnace door brick uniform, promote the transformation of the internal quartz crystals through the mineralizer, and generate fine and uniform pores inside the brick body, so that the final furnace door brick has good thermal insulation performance, high strength and excellent corrosion resistance.
[0035] (2) The composite mineralizer of the present invention generates calcium alginate through sodium alginate and calcium chloride. Calcium alginate is combined with nano-silicon dioxide to form silica hybridized calcium alginate. The formation of calcium alginate is promoted by cold and hot cycles. The silica hybridized calcium alginate and other components work together to promote the conversion of quartz crystals to tridymite during sintering, reduce the residual quartz content, and make the furnace door bricks have fine and uniform pores inside after sintering, thereby improving the thermal insulation performance of the furnace door bricks. DETAILED DESCRIPTION
[0036] The present invention is further described in detail below in conjunction with specific implementation methods to better reflect the advantages of the present invention.
[0037] Example 1
[0038] Energy-saving coke oven door bricks with enhanced thermal insulation and corrosion resistance, the raw materials of the door bricks comprising, by weight: 80 parts of silica, 3 parts of composite mineralizer, 5 parts of binder, and 4 parts of additive;
[0039] The silica comprises, by mass percentage, 60% silica aggregate, 15% silica coarse powder, and the rest silica fine powder, wherein the particle size of the silica aggregate is 2-3 mm, the particle size of the silica coarse powder is 400-450 μm, and the particle size of the silica fine powder is 8-15 μm;
[0040] The composite mineralizer comprises, by weight: 0.90 parts of fluorite powder, 0.10 parts of iron phosphorus, 1.50 parts of calcium chloride, 0.40 parts of sodium alginate, and 0.10 parts of nano silicon dioxide;
[0041] The binder is sulfite paper waste slurry with a specific gravity of 1.2 g / ml; the additive is silicon carbide;
[0042] The preparation method of the composite mineralizer is:
[0043] S1: Add nano-silicon dioxide to deionized water and disperse by ultrasonic for 6 minutes to obtain a nano-silicon dioxide dispersion with a mass concentration of 6%;
[0044] S2: adding sodium alginate to deionized water to prepare a sodium alginate gel solution with a mass concentration of 5%, and then diluting the sodium alginate gel solution by 15 times to obtain a sodium alginate diluted solution;
[0045] S3: using a planetary ball mill to uniformly mix fluorite powder, iron phosphorus and calcium chloride to obtain a mixed powder, wherein the ball-to-material ratio of the planetary ball mill is 2:1 and the ball milling time is 20 minutes;
[0046] S4: stirring the sodium alginate dilution liquid, and subjecting the sodium alginate dilution liquid to a hot and cold cycle between a high temperature and a low temperature, wherein the high temperature is 35°C, the low temperature is 3°C, and the temperature change rate during the hot and cold cycle is 5°C / min. During the hot and cold cycle, when the temperature of the sodium alginate dilution liquid rises to a high temperature, a nano-silicon dioxide dispersion liquid is added to the sodium alginate dilution liquid once, and when the temperature of the sodium alginate dilution liquid drops to 12°C, a mixed powder is added to the sodium alginate dilution liquid once; the single addition amount of the nano-silicon dioxide dispersion liquid accounts for 20% of the total amount thereof; the single addition amount of the mixed powder accounts for 25% of its weight, until the nano-silicon dioxide dispersion liquid and the mixed powder are all added to the sodium alginate dilution liquid to obtain a mixed liquid;
[0047] S5: filtering, crushing and drying the solid particles in the mixed solution in sequence to obtain a composite mineralizer, wherein the particle size of the solid particles after crushing is ≤125 μm;
[0048] On the other hand, the preparation method of the furnace door brick comprises the following steps:
[0049] Step 1: Add silica aggregate, silica coarse powder and silica fine powder to a wet mill in sequence, dry mix for 4 minutes, add additives and composite mineralizer to the wet mill, then add a binder and mix for 12 minutes, and obtain mud after mixing;
[0050] Step 2: using a press to press the mud into a brick, and then drying the brick at 230° C. for 21 hours to obtain a dried brick;
[0051] Step 3: Place the dried bricks into a tunnel kiln and heat them to 1420°C for firing. The firing time is 84 hours. After the firing is completed, furnace door bricks are obtained. The heating process is: first increase the temperature to 720°C at a heating rate of 22°C / h, then increase the temperature to 1050°C at a heating rate of 17°C / h, and then increase the temperature to 1280°C at a heating rate of 7°C / h. After keeping warm for 1.5 hours, increase the temperature to 1420°C at a heating rate of 3°C / h.
[0052] Example 2
[0053] This embodiment is basically the same as the embodiment 1, except that the raw materials of the furnace door bricks include, by weight: 70 parts of silica, 1 part of composite mineralizer, 3 parts of binder, and 2 parts of additives.
[0054] Example 3
[0055] This embodiment is basically the same as the embodiment 1, except that the raw materials of the furnace door bricks include, by weight: 85 parts of silica, 5 parts of composite mineralizer, 8 parts of binder, and 6 parts of additive.
[0056] Example 4
[0057] This embodiment is basically the same as Embodiment 1, except that the silica comprises, by mass percentage, 50% silica aggregate, 10% silica coarse powder, and the rest silica fine powder, wherein the particle size of the silica aggregate is 1 to 2 mm, the particle size of the silica coarse powder is 340 to 400 μm, and the particle size of the silica fine powder is 5 to 8 μm.
[0058] Example 5
[0059] This embodiment is basically the same as Embodiment 1, except that the silica comprises, by mass percentage, 70% silica aggregate, 20% silica coarse powder, and the rest silica fine powder, wherein the particle size of the silica aggregate is 4 to 4.5 mm, the particle size of the silica coarse powder is 450 to 500 μm, and the particle size of the silica fine powder is 15 to 20 μm.
[0060] Example 6
[0061] This embodiment is basically the same as Embodiment 1, except that the composite mineralizer comprises, by weight: 0.35 parts of fluorite powder, 0.03 parts of iron phosphorus, 0.55 parts of calcium chloride, 0.04 parts of sodium alginate, and 0.03 parts of nano-silicon dioxide.
[0062] Example 7
[0063] This embodiment is basically the same as Embodiment 1, except that the composite mineralizer comprises, by weight: 1.60 parts of fluorite powder, 0.35 parts of iron phosphorus, 1.90 parts of calcium chloride, 0.80 parts of sodium alginate, and 0.35 parts of nano-silicon dioxide.
[0064] Example 8
[0065] This embodiment is basically the same as the embodiment 1, except that the mass concentration of the nano-silicon dioxide dispersion is 5%, and the sodium alginate gel is diluted 10 times.
[0066] Example 9
[0067] This embodiment is basically the same as the embodiment 1, except that the mass concentration of the nano-silicon dioxide dispersion is 8%, and the sodium alginate gel is diluted 20 times.
[0068] Example 10
[0069] This embodiment is basically the same as the embodiment 1, except that the temperature of the sodium alginate dilution solution is subjected to a hot and cold cycle between a high temperature and a low temperature, wherein the high temperature is 30° C. and the low temperature is 0° C.
[0070] Embodiment 11
[0071] This embodiment is basically the same as the embodiment 1, except that the temperature of the sodium alginate dilution solution is subjected to a hot and cold cycle between a high temperature and a low temperature, wherein the high temperature is 40°C and the low temperature is 6°C.
[0072] Example 12
[0073] This embodiment is basically the same as Embodiment 1, except that the temperature change rate during the hot and cold cycle is 3°C / min.
[0074] Example 13
[0075] This embodiment is basically the same as Embodiment 1, except that the temperature change rate during the hot and cold cycle is 6°C / min.
[0076] Embodiment 14
[0077] This embodiment is substantially the same as the embodiment 1, except that when the temperature of the sodium alginate dilution solution drops to 10° C., the primary mixed powder is added to the sodium alginate dilution solution.
[0078] Embodiment 15
[0079] This embodiment is substantially the same as the embodiment 1, except that when the temperature of the sodium alginate dilution solution drops to 15° C., the primary mixed powder is added to the sodium alginate dilution solution.
[0080] Example 16
[0081] This embodiment is basically the same as embodiment 1, except that the initial addition amount of the nano-silicon dioxide dispersion accounts for 15% of the total amount, the part less than 15% is added in full, and the initial addition amount of the mixed powder accounts for 20% of its weight.
[0082] Embodiment 17
[0083] This embodiment is basically the same as embodiment 1, except that the initial addition amount of the nano-silicon dioxide dispersion accounts for 25% of the total amount; the initial addition amount of the mixed powder accounts for 30% of its weight, and the part less than 30% is added in full.
[0084] Embodiment 18
[0085] This embodiment is basically the same as Embodiment 1, except that the temperature rise process is as follows: first, the temperature rises to 700°C at a temperature rise rate of 20°C / h, then rises to 1000°C at a temperature rise rate of 15°C / h, then rises to 1250°C at a temperature rise rate of 5°C / h, and after keeping warm for 1 hour, rises to 1380°C at a temperature rise rate of 2°C / h.
[0086] Embodiment 19
[0087] This embodiment is basically the same as Embodiment 1, except that the temperature rises to 750°C at a rate of 25°C / h, then to 1100°C at a rate of 20°C / h, then to 1300°C at a rate of 10°C / h, and after keeping warm for 2 hours, the temperature is raised to 1480°C at a rate of 5°C / h.
[0088] Experimental example
[0089] The thermal conductivity of the furnace door bricks prepared in each embodiment at 1000°C was tested respectively, and the furnace door bricks prepared in each embodiment were ground into pieces of the same size, and the pieces obtained in each embodiment were corroded in sulfuric acid with a mass concentration of 30% for 12 hours. During the corrosion process, the sulfuric acid was heated to 90°C, and the mass loss of the pieces obtained in each embodiment before and after corrosion was calculated to explore the corrosion resistance of the furnace door bricks. The specific exploration is as follows:
[0090] 1. Explore the influence of raw material ratio on the performance of furnace door bricks
[0091] Using Examples 1, 2, and 3 as experimental comparisons, and selecting commercially available common silica bricks as Comparative Example 1, the performance of furnace door bricks under different raw material ratios is shown in Table 1 below:
[0092] Table 1 Performance of furnace door bricks under different ratios of raw materials
[0093] Group Thermal conductivity (W / mK) Mass loss (%) Example 1 0.56 1.35 Example 2 0.62 1.54 Example 3 0.64 1.58 Comparative Example 1 1.42 1.89
[0094] It can be seen from the data of Mark 1 that compared with Examples 1, 2, and 3, the furnace door bricks of Example 1 have the lowest thermal conductivity and the smallest mass loss, indicating that the furnace door bricks of Example 1 have the best thermal insulation performance and corrosion resistance, and the raw material ratio selected in Example 1 is optimal; compared with Comparative Example 1, the furnace door bricks of Example 1 have lower thermal conductivity and smaller mass loss, indicating that the furnace door bricks of Example 1 have better thermal insulation performance and corrosion resistance than commercially available silica bricks.
[0095] 2. Investigate the influence of silica parameters on the performance of furnace door bricks
[0096] Examples 1, 4, and 5 were used as experimental comparisons. Example 1 was used as a reference. All silica aggregates with a particle size of 2 to 3 mm were used as comparative example 2. The furnace door brick performance under different silica parameters was shown in Table 2 below:
[0097] Table 2 Performance of furnace door bricks under different silica parameters
[0098] Group Thermal conductivity (W / mK) Mass loss (%) Example 1 0.56 1.35 Example 4 0.62 1.52 Example 5 0.69 1.65 Comparative Example 2 1.12 1.95
[0099] It can be seen from the data in Table 2 that compared with Examples 1, 4, and 5, the furnace door bricks of Example 1 have the lowest thermal conductivity and the smallest mass loss, indicating that the furnace door bricks of Example 1 have the best thermal insulation performance and corrosion resistance, and the silica parameters selected in Example 1 are optimal; compared with Comparative Example 2, Example 1 has a lower thermal conductivity and a smaller mass loss, indicating that the furnace door bricks of Example 1 have better thermal insulation performance and corrosion resistance than Comparative Example 2, and the silica parameters selected in Example 1 are better.
[0100] 3. Investigate the influence of composite mineralizer ratio on the performance of furnace door bricks
[0101] Examples 1, 6, and 7 were used as experimental comparisons. Example 1 was used as a reference, and sodium alginate in the composite mineralizer was removed as comparative example 3. The furnace door brick properties under different ratios of the composite mineralizer were shown in Table 3 below:
[0102] Table 3 Performance of furnace door bricks under different ratios of composite mineralizer
[0103]
[0104]
[0105] It can be seen from the data in Table 3 that compared with Examples 1, 6 and 7, the furnace door brick of Example 1 has the lowest thermal conductivity and the smallest mass loss, indicating that the furnace door brick of Example 1 has the best thermal insulation performance and corrosion resistance, and the composite mineralizer ratio selected in Example 1 is optimal; compared with Comparative Example 3, the furnace door brick of Example 1 has lower thermal conductivity and smaller mass loss, indicating that after sodium alginate is removed from the composite mineralizer, the thermal insulation performance and corrosion resistance of the furnace door brick are reduced.
[0106] 4. Investigate the effect of nano-silicon dioxide dispersion and sodium alginate glue concentration on the performance of furnace door bricks
[0107] Using Examples 1, 8, and 9 as experimental comparisons, the furnace door brick performances at different concentrations of nano-silicon dioxide dispersion and sodium alginate glue are shown in Table 4 below:
[0108] Table 4 Performance of furnace door bricks at different concentrations of nano-silicon dioxide dispersion and sodium alginate glue
[0109] Group Thermal conductivity (W / mK) Mass loss (%) Example 1 0.56 1.35 Example 8 0.61 1.40 Example 9 0.66 1.43
[0110] It can be seen from the data in Table 4 that the furnace door bricks of Example 1 have the lowest thermal conductivity and the smallest mass loss, indicating that the furnace door bricks of Example 1 have the best thermal insulation performance and corrosion resistance, and the concentrations of the nano-silicon dioxide dispersion and the sodium alginate glue selected in Example 1 are optimal.
[0111] 5. Explore the influence of hot and cold cycle temperature on the performance of furnace door bricks
[0112] Examples 1, 10, and 11 were used as experimental comparisons. Example 1 was used as a reference. The temperature of the sodium alginate dilution solution did not change, and the nano-silicon dioxide dispersion and the mixed powder were added in one go as comparative example 4. The furnace door brick performance at different hot and cold cycle temperatures was shown in Table 5 below:
[0113] Table 5 Performance of furnace door bricks at different hot and cold cycle temperatures
[0114] Group Thermal conductivity (W / mK) Mass loss (%) Example 1 0.56 1.35 Example 10 0.65 1.51 Embodiment 11 0.63 1.45 Comparative Example 4 0.98 1.72
[0115] It can be seen from the data in Table 5 that compared with Examples 1, 10 and 11, the furnace door bricks of Example 1 have the lowest thermal conductivity and the smallest mass loss, indicating that the furnace door bricks of Example 1 have the best thermal insulation performance and corrosion resistance, and the hot and cold cycle temperature selected by Example 1 is optimal; compared with Comparative Example 4, the furnace door bricks of Example 1 have lower thermal conductivity and smaller mass loss, indicating that the furnace door bricks of Example 1 have better thermal insulation performance and corrosion resistance, and the nano-silicon dioxide dispersion and mixed powder addition method of Example 1 is better.
[0116] 6. Investigate the effect of temperature change rate during hot and cold cycles on the performance of furnace door bricks
[0117] Using Examples 1, 12, and 13 as experimental comparisons, the furnace door brick performance at different temperature change rates during hot and cold cycles is shown in Table 6 below:
[0118] Table 6 Performance of furnace door bricks at different temperature change rates during hot and cold cycles
[0119] Group Thermal conductivity (W / mK) Mass loss (%) Example 1 0.56 1.35 Example 12 0.68 1.49 Example 13 0.66 1.47
[0120] It can be seen from the data in Table 6 that the furnace door bricks of Example 1 have the lowest thermal conductivity and the smallest mass loss, indicating that the furnace door bricks of Example 1 have the best thermal insulation performance and corrosion resistance, and the temperature change rate during the hot and cold cycle selected by Example 1 is optimal.
[0121] 7. Investigate the effect of sodium alginate dilution temperature on the performance of furnace door bricks when adding mixed powder
[0122] Using Examples 1, 14 and 15 as experimental comparisons, the furnace door brick performance at different temperatures of sodium alginate dilution when the mixed powder is added is shown in Table 7 below:
[0123] Table 7 Furnace door brick properties at different temperatures of sodium alginate dilution when adding mixed powder
[0124] Group Thermal conductivity (W / mK) Mass loss (%) Example 1 0.56 1.35 Embodiment 14 0.59 1.39 Embodiment 15 0.62 1.44
[0125] It can be seen from the data in Table 7 that the furnace door bricks of Example 1 have the lowest thermal conductivity and the smallest mass loss, indicating that the furnace door bricks of Example 1 have the best thermal insulation performance and corrosion resistance, and the temperature of the sodium alginate dilution solution selected in Example 1 when adding the mixed powder is optimal.
[0126] 8. Investigate the effect of single addition amount of nano-silicon dioxide dispersion and mixed powder on the performance of furnace door bricks
[0127] Using Examples 1, 16, and 17 as experimental comparisons, the furnace door brick performances obtained under different single addition amounts of nano-silicon dioxide dispersion and mixed powder are shown in Table 8 below:
[0128] Table 8 Performance of furnace door bricks at different single addition amounts of nano-silicon dioxide dispersion and mixed powder
[0129]
[0130]
[0131] It can be seen from the data in Table 8 that the furnace door bricks in Example 1 have the lowest thermal conductivity and the smallest mass loss, indicating that the furnace door bricks in Example 1 have the best thermal insulation performance and corrosion resistance, and the single addition amount of the silicon dioxide dispersion and mixed powder selected in Example 1 is optimal.
[0132] 9. Explore the influence of heating parameters on the performance of furnace door bricks during sintering
[0133] Examples 1, 18, and 19 were used as experimental comparisons. Example 1 was used as a reference. The entire heating process was performed at 20°C / h as comparative example 5. The furnace door brick performance under different heating parameters was shown in Table 9 below:
[0134] Table 9 Performance of furnace door bricks under different heating parameters
[0135] Group Thermal conductivity (W / mK) Mass loss (%) Example 1 0.56 1.35 Embodiment 18 0.68 1.52 Embodiment 19 0.64 1.46 Comparative Example 5 0.93 1.89
[0136] It can be seen from the data in Table 9 that compared with Examples 1, 18 and 19, the furnace door bricks of Example 1 have the lowest thermal conductivity and the smallest mass loss, indicating that the furnace door bricks of Example 1 have the best thermal insulation performance and corrosion resistance, and the heating parameters selected in Example 1 are optimal; compared with Comparative Example 5, the furnace door bricks of Example 1 have lower thermal conductivity and smaller mass loss, indicating that the furnace door bricks of Example 1 have better thermal insulation performance and corrosion resistance, and the heating method selected in Example 1 is better.
Claims
1. Energy-saving coke oven door bricks with enhanced thermal insulation and corrosion resistance, It is characterized in that The raw materials of the furnace door bricks include, by weight: 70-85 parts of silica, 1-5 parts of composite mineralizer, 3-8 parts of binder, and 2-6 parts of additives; The silica comprises, by mass percentage, 50-70% silica aggregate, 10-20% silica coarse powder, and the rest silica fine powder, wherein the particle size of the silica aggregate is 1-4.5 mm, the particle size of the silica coarse powder is 340-500 μm, and the particle size of the silica fine powder is 5-20 μm; The composite mineralizer comprises, by weight: 0.35-1.60 parts of fluorite powder, 0.03-0.35 parts of iron phosphorus, 0.55-1.90 parts of calcium chloride, 0.04-0.80 parts of sodium alginate, and 0.03-0.35 parts of nano silicon dioxide; The binder is sulfite paper waste pulp with a specific gravity of 1.18 to 1.28 g / ml; The additive is a mixture of any one or more of silicon carbide or silicon nitride in any ratio; The preparation method of the composite mineralizer is: S1: adding nano-silicon dioxide to deionized water, and ultrasonically dispersing for 5 to 8 minutes to obtain a nano-silicon dioxide dispersion with a mass concentration of 5 to 8%; S2: adding sodium alginate to deionized water to prepare a sodium alginate gel solution with a mass concentration of 5%, and then diluting the sodium alginate gel solution by 10 to 20 times to obtain a sodium alginate diluted solution; S3: using a planetary ball mill to uniformly mix fluorite powder, iron phosphorus and calcium chloride to obtain a mixed powder; S4: stirring the sodium alginate dilution liquid, and subjecting the sodium alginate dilution liquid to a hot and cold cycle between a high temperature and a low temperature, wherein the high temperature is 30-40° C. and the low temperature is 0-6° C. During the hot and cold cycle, when the temperature of the sodium alginate dilution liquid rises to a high temperature, a nano-silicon dioxide dispersion liquid is added to the sodium alginate dilution liquid once, and when the temperature of the sodium alginate dilution liquid drops to 10-15° C., a mixed powder is added to the sodium alginate dilution liquid once; the single addition amount of the nano-silicon dioxide dispersion liquid accounts for 15-25% of the total amount thereof; the single addition amount of the mixed powder accounts for 20-30% of its weight, until the nano-silicon dioxide dispersion liquid and the mixed powder are all added to the sodium alginate dilution liquid to obtain a mixed liquid; S5: filtering, crushing and drying the solid particles in the mixed solution in sequence to obtain a composite mineralizer; In step S3, the ball-to-material ratio of the planetary ball mill is 1-3:1, and the ball milling time is 10-25 min; In step S4, the temperature change rate during the hot and cold cycle is 3-6°C / min; In step S5, the solid particles are crushed to a particle size of ≤125 μm.
2. The method for preparing furnace door bricks according to claim 1, It is characterized in that The following steps are involved: Step 1: Add silica aggregate, silica coarse powder and silica fine powder to a wet mill in sequence, dry mix for 3 to 5 minutes, add additives and composite mineralizers to the wet mill, then add a binder and mix for 10 to 15 minutes, and obtain mud after mixing; Step 2: using a press to press the mud into a brick, and then drying the brick at 220-240° C. for 20-22 hours to obtain a dried brick; Step 3: Place the dried bricks into a tunnel kiln and heat them to 1380-1480°C for firing. The firing time is 82-85 hours. After firing, furnace door bricks are obtained.
3. The method for preparing the energy-saving coke oven door brick with enhanced thermal insulation and corrosion resistance according to claim 2, It is characterized in that In step 3, the heating process is as follows: first, the temperature is increased to 700-750°C at a heating rate of 20-25°C / h, then increased to 1000-1100°C at a heating rate of 15-20°C / h, then increased to 1250-1300°C at a heating rate of 5-10°C / h, and after keeping warm for 1-2h, the temperature is increased to 1380-1480°C at a heating rate of 2-5°C / h.