A method for preparing nanofiber silica by biomineralization of actin

The nanofiber silica is synthesized at room temperature through actin biomineralization technology, which solves the problems of high temperature and high pressure and harmful by-products in the existing process, and realizes low-cost and environmentally friendly nanofiber silica preparation with adjustable control nanostructures and nanotube structures.

CN117448986BActive Publication Date: 2024-11-19WUHAN UNIV OF TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202311507075.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-10
Publication Date
2024-11-19
Estimated Expiration
2043-11-10

AI Technical Summary

Technical Problem

The conventional manufacturing processes of existing silica nanomaterials require harsh conditions such as high temperature and high pressure, extreme pH, etc., and have limited control over morphology and structure. Accompanied by-products, low-cost and environmentally friendly biosynthesis methods are lacking.

Method used

Actin is used as a biological template, through the polymerization and mineralization process at room temperature, tetraethyl orthosilicate is used to regulate the solution pH under the action of fibrous actin to achieve the biosynthesis of nanofiber silica, forming a nanotube structure .

Benefits of technology

It realizes the preparation of nanofiber silica with low cost, simple operation, energy-saving and environmentally friendly, with a tunable nanostructure, and has opened up new channels for biomineralization and synthesis. The prepared silica has excellent nanotube structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117448986B_ABST
    Figure CN117448986B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing nano-fiber silica by biomineralization of actin, comprising the following steps: S1, polymerizing monomer actin into fibrous actin: adding 1 to 2 volumes of polymerization buffer to a monomer actin solution, uniformly stirring, polymerizing at room temperature for a certain period of time to obtain fibrous actin; S2, synthesizing nano-fiber silica guided by fibrous actin: adding 0.1 to 0.2 volumes of tetraethyl orthosilicate to the fibrous actin solution in step S1, regulating the pH of the solution, mineralizing at room temperature, and freeze-drying to obtain fibrous silica. The nano-fiber silica of the present invention has low preparation cost, simple operation, energy saving and environmental protection, and a controllable structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to new materials and application fields thereof, and more specifically to a method for preparing nano-fiber silicon dioxide by biomineralization of actin. Background Art

[0002] The structural formation process of natural substances is the result of billions of years of evolution and natural selection. Usually, natural substances can complete the structural formation process at room temperature, grow exquisite microstructures, and obtain unique functions. In modern industry, the preparation methods of materials with similar properties often require high temperatures and other conditions. In recent years, the international community has reported the direct use of living organisms to construct a natural synthesis platform, realizing the controllable preparation of inorganic materials in vivo at room temperature.

[0003] Jingjing Xie et al. used pearl-producing freshwater mussels as a mineralization synthesis platform to synthesize nitrogen-doped anatase TiO2 with a hierarchical pore structure at room temperature, and the powder had excellent photodegradation and photohydrogen production performance. Through mass spectrometry analysis, it was found that the proteins in the TiO2 nanopowder were almost all intracellular proteins that constitute the cell composition, rather than the extracellular proteins secreted by traditional cells, among which actin that constitutes the cytoskeleton was the most abundant (Jingjing Xie, et al. Mussel-Directed Synthesis of Nitrogen-Doped Anatase TiO2 [J]. Angewandte Chemie, 2016.). Hui Zeng et al. used the extracellular protein mantle fluid protein to regulate inorganic materials in vitro and found that although the mantle fluid protein does not have the ability to guide the room temperature crystallization of TiO2, it has the function of regulating the crystal form and morphology of TiO2 at a certain temperature (Hui Zeng, et al. Bioprocess-inspired synthesis of hierarchically porous nitrogen-doped TiO2 with high visible-light photocatalytic activity [J]. Journal of Materials Chemistry, A. 2015.). Previous studies have shown that intracellular and extracellular proteins have different regulatory mechanisms on the growth of inorganic materials. However, the mechanism of intracellular proteins, especially actin, in guiding the synthesis of inorganic materials has not been reported. Therefore, it is necessary to study the mechanism of action between intracellular proteins and inorganic materials, clarify the key control factors for organisms to guide the room temperature synthesis of inorganic materials, and provide important basic technical support for the room temperature preparation of high-performance inorganic materials in vitro.

[0004] Silica-based nanomaterials have been extensively studied for many years because of their potential applications in a variety of technologies such as catalysis, sensing, separation, enzyme immobilization, and gene and drug delivery. Conventional manufacturing processes for silica nanomaterials usually require harsh conditions such as high temperature and pressure, extreme pH values, and the extensive use of hazardous reagents and solvents. In addition, these chemical-based manufacturing processes usually have relatively limited control over the morphology and structure of the resulting silica nanomaterials and are accompanied by harmful byproducts. In contrast, many organisms synthesize a large amount of silica nanomaterials under benign reaction conditions, namely ambient temperature and pressure and neutral pH. Bio-silica nanomaterials are often superior to most existing artificial materials in terms of formation process, structure and performance. Therefore, exploring the biosynthesis of silica in combination with intracellular proteins is of great guiding significance for better control of nano-silica production.

[0005] Existing research mainly focuses on the synthesis of inorganic materials by extracellular proteins. However, there are different regulatory mechanisms between intracellular and extracellular proteins on the growth of inorganic materials, especially the mechanism of intracellular protein actin in guiding the synthesis of inorganic materials has not been reported. The conventional manufacturing process of silica nanomaterials usually requires harsh conditions such as high temperature, high pressure, and extreme pH values, and the morphology and structure of the resulting silica nanomaterials are limited, and are accompanied by harmful byproducts. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a method for preparing nanofiber silica by biomineralization of actin, wherein the nanofiber silica has low preparation cost, simple operation, energy saving and environmental protection, and controllable structure.

[0007] The technical solution adopted by the present invention to solve the technical problem is: constructing a method for preparing nanofiber silica by biomineralization of actin, comprising the following steps:

[0008] S1. Polymerizing monomeric actin into fibrous actin: adding 1 to 2 times the volume of polymerization buffer to the monomeric actin solution, stirring evenly, and polymerizing at room temperature for a certain period of time to obtain fibrous actin;

[0009] S2. Synthesis of nanofibrous silica under the guidance of fibrous actin: adding 0.1 to 0.2 volumes of tetraethyl orthosilicate to the fibrous actin solution in step S1, adjusting the pH of the solution, mineralizing at room temperature, and freeze-drying to obtain fibrous silica.

[0010] According to the above scheme, in step S1, the molecular weight of actin is 42-43 kDa.

[0011] According to the above scheme, in step S1, the actin concentration in the solution is 4-7 mg / mL.

[0012] According to the above scheme, in step S1, the polymerization buffer in the solution includes the following components: 40-50 mM / L Tris-HCL, 1.0-1.5 mM / L ATP, 1.0-1.5 mM / L DTT, 1.0-1.5 mM / L MgCl2, 15-20 mM / L CaCl2, and the pH of the buffer solution is 7.0-8.0.

[0013] According to the above scheme, in step S1, the stirring time is 3 minutes, and the polymerization time at room temperature is 4 to 6 hours.

[0014] According to the above scheme, in step S2, the concentration of tetraethyl orthosilicate is 0.75M / L.

[0015] According to the above scheme, in step S2, the pH of the solution is regulated to be 4.0 to 9.0, the room temperature mineralization time is 5 to 7 days, and the freeze-drying time is 12 to 24 hours.

[0016] The method for preparing nanofiber silica by biomineralization of actin of the present invention has the following characteristics:

[0017] Beneficial effects:

[0018] 1. The present invention hydrolyzes tetraethyl orthosilicate in a solution, and the hydrolyzate is deposited, polymerized, and grown under the regulation of fibrous actin with a biological template and a structure-directing agent, and finally forms fibrous silica;

[0019] 2. The silicon dioxide prepared by the present invention has a nanofiber structure and a nanochannel structure, and the controllability of the silicon dioxide nanostructure can be achieved by changing the pH of the solution;

[0020] 3. The present invention successfully polymerizes monomeric actin into fibrous actin, and successfully utilizes the fibrous actin to achieve the regulation of the biomineralization process of silicon dioxide, opening up a new channel for the synthesis of silicon dioxide;

[0021] 4. The preparation method of the present invention is simple and easy to operate, has low preparation cost and mild reaction conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The present invention will be further described below with reference to the accompanying drawings and embodiments, in which:

[0023] Figure 1 This is the protein electrophoresis diagram of actin in Example 1 of the present invention,

[0024] Among them: the first column is actin,

[0025] The second column is Marker;

[0026] Figure 2The XRD patterns of the nanofiber silica prepared in Example 1, Example 2 and Example 3 of the present invention are as follows:

[0027] Wherein: a-XRD spectrum of nanofiber silica prepared in Example 1,

[0028] b- XRD spectrum of nanofiber silica prepared in Example 2,

[0029] c-XRD spectrum of nanofiber silica prepared in Example 3);

[0030] Figure 3 This is a SEM image of the nanofiber silica prepared in Example 1 of the present invention;

[0031] Figure 4 This is a SEM image of nanofiber silica prepared in Example 2 of the present invention;

[0032] Figure 5 This is a SEM image of nanofiber silica prepared in Example 3 of the present invention;

[0033] Figure 6 This is a TEM image of nanofiber silica prepared in Example 3 of the present invention;

[0034] Figure 7 This is a SEM image of nano-silicon dioxide prepared in Comparative Example 1 of the present invention;

[0035] Figure 8 This is a SEM image of nano-silicon dioxide prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0036] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, specific embodiments of the present invention are now described in detail with reference to the accompanying drawings.

[0037] like Figure 1-6As shown, a method for preparing nano-fiber silica by biomineralization of actin of the present invention comprises the following steps: S1, polymerizing monomer actin into fibrous actin: adding 1 to 2 volumes of polymerization buffer to a monomer actin solution, stirring evenly, and polymerizing for a certain period of time at room temperature to obtain fibrous actin; the molecular weight of actin is 42 to 43 kDa; the actin concentration in the solution is 4 to 7 mg / mL; the polymerization buffer in the solution comprises the following components: 40 to 50 mM / L Tris-HCL, 1.0 to 1.5 mM / L ATP, 1.0 to 1.5 mM / L DTT, 1.0 to 1.5 mM / L MgCl2, 15 to 20 mM / L CaCl2, and the pH of the buffer solution is 7.0 to 8.0; the stirring time is 3 min, and the polymerization time at room temperature is 4 to 6 h. S2. Synthesis of nanofibrous silica under the guidance of fibrous actin: add 0.1-0.2 volume of tetraethyl orthosilicate to the fibrous actin solution in step S1, adjust the pH of the solution, mineralize at room temperature, and obtain fibrous silica by freeze-drying; the concentration of tetraethyl orthosilicate is 0.75 M / L; adjust the pH of the solution to 4.0-9.0, the mineralization time at room temperature is 5-7 days, and the freeze-drying time is 12-24 hours.

[0038] Example 1

[0039] A method for preparing nanofiber silica by biomineralization of actin comprises the following steps:

[0040] Step 1: Prepare a 4 mg / mL monomer actin solution, add a polymerization buffer of 50 mM Tris-HCL, pH 7.5, 1 mM ATP, 1 mM DTT, 1 mM MgCl2, and 20 mM CaCl2, stir at room temperature for 3 min, and then polymerize and cross-link for 4 h to obtain a fibrous actin solution.

[0041] Step 2: Add 0.75 M tetraethyl orthosilicate to the solution obtained in step 1, adjust the pH value of the solution to 4.0, stir for 3 minutes, mineralize at room temperature for 5 days, and freeze-dry for 24 hours to obtain fibrous silica.

[0042] like Figure 1 As shown, the purity of the actin solution prepared in this example was detected by protein gel electrophoresis, and the molecular weight of actin was 43kDa. The results showed that the prepared solution contained pure actin. The mineralization product was detected by XRD and SEM. The XRD results are shown in Figure 2 As shown in the curve a, the results show that the synthesized silica is an amorphous phase. Figure 3 As shown, the results show that the synthesized silica is a fiber structure assembled from particles of about 10 nm, and the fiber diameter is about 150 nm.

[0043] Example 2

[0044] A method for preparing nanofiber silica by biomineralization of actin comprises the following steps:

[0045] Step 1: Prepare a 7 mg / mL monomer actin solution, add a polymerization buffer of 50 mM Tris-HCL, pH 7.5, 1 mM ATP, 1 mM DTT, 1 mM MgCl2, and 20 mM CaCl2, stir at room temperature for 3 min, and then polymerize and cross-link for 6 h to obtain a fibrous actin solution.

[0046] Step 2: Add 0.75 M tetraethyl orthosilicate to the solution obtained in step 1, adjust the pH value of the solution to 7.0, stir for 3 minutes, mineralize at room temperature for 7 days, and freeze-dry for 24 hours to obtain fibrous silica.

[0047] The mineralization products were detected by XRD and SEM. The XRD results are as follows Figure 2 As shown in the curve b, the results show that the synthesized silica is an amorphous phase. Figure 4 As shown, the results show that the synthesized silica is a fiber structure assembled from particles of about 20 nm, and the fiber diameter is about 150 nm.

[0048] Example 3

[0049] A method for preparing nanofiber silica by biomineralization of actin comprises the following steps:

[0050] Step 1: Prepare a 4 mg / mL monomer actin solution, add polymerization buffer 50 mM Tris-HCL, pH 7.5, 1 mM ATP, 1 mM DTT, 1 mM MgCl2, 20 mM CaCl2, stir at room temperature for 3 min, and then cross-link for 6 h to obtain a fibrous actin solution.

[0051] Step 2: Add 0.75 M tetraethyl orthosilicate to the solution obtained in step 1, adjust the pH value of the solution to 9.0, stir for 3 minutes, mineralize at room temperature for 7 days, and freeze-dry for 12 hours to obtain fibrous silica.

[0052] The mineralization products were detected by XRD, SEM and TEM. The XRD results are as follows Figure 2 As shown in the curve c, the results show that the synthesized silica is an amorphous phase. Figure 5 As shown in Figure 1, the results show that the synthesized silica is a fiber structure assembled from particles of about 50 nm, with a fiber diameter of about 200 nm. Figure 6As shown, the results show that the synthesized fibrous silica has a channel structure inside, and the channel diameter is about 5nm.

[0053] Comparative Example 1

[0054] The method for preparing nano silicon dioxide with pure aqueous solution comprises the following steps:

[0055] Step 1: Add polymerization buffer 50 mM Tris-HCL, pH 7.5, 1 mM ATP, 1 mM DTT, 1 mM MgCl2, 20 mM CaCl2 to the pure water solution. Stir at room temperature for 3 min and then let stand for 6 h.

[0056] Step 2: Add 0.75 M tetraethyl orthosilicate to the solution obtained in step 1, adjust the pH value of the solution to 4.0, stir for 3 minutes, mineralize at room temperature for 7 days, and freeze-dry for 12 hours to obtain nano-silicon dioxide.

[0057] The mineralization products were detected by SEM. Figure 7 As shown, the results show that the synthesized product is an agglomerate of silica particles with a particle size of about 10 nm, and a fiber structure cannot be obtained under this condition.

[0058] Comparative Example 2

[0059] The method for preparing nano silicon dioxide with pure aqueous solution comprises the following steps:

[0060] Step 1: Add polymerization buffer 40 mM Tris-HCL, pH 7.5, 1 mM ATP, 1 mM DTT, 1 mM MgCl2, 15 mM CaCl2 to the pure water solution. Stir at room temperature for 3 min and then let stand for 6 h.

[0061] Step 2: Add 0.75 M tetraethyl orthosilicate to the solution obtained in step 1, adjust the pH value of the solution to 9.0, stir for 3 minutes, mineralize at room temperature for 7 days, and freeze-dry for 12 hours to obtain nano-silicon dioxide.

[0062] The mineralization products were detected by SEM. Figure 8 As shown, the results show that the synthesized product is silica particles with a particle size of about 100 nm, and a fiber structure cannot be obtained under this condition.

[0063] In summary, in the above-mentioned Examples 1 to 3, actin is used to regulate the synthesis of silica, and a novel nanofiber structure is prepared, the diameter of which is about 200 nm, and there are multiple tubes with a diameter of about 5 nm inside the fiber. The microstructure of the silica mineralization product can be regulated by changing the pH value of the solution. However, in Comparative Examples 1 to 2, the synthesized products under pure water solution are silica nanoparticles, and no fiber structure can be obtained. The results show the importance of actin in the synthesis of fibrous silica. This work has opened up a new channel for the biomineralization synthesis of silica materials.

[0064] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above-mentioned specific implementation modes, which are merely illustrative rather than restrictive. Under the guidance of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the present invention and the claims, all of which are within the protection of the present invention.

Claims

1. A method for preparing nanofiber silica by biomineralization of actin, characterized in that: The following steps are involved: S1. Polymerization of monomeric actin into fibrous actin: Add 1-2 times the volume of polymerization buffer to the monomeric actin solution, stir evenly, and polymerize at room temperature for a certain period of time to obtain fibrous actin; The polymerization buffer in the solution includes the following components: 40~50 mM / L Tris-HCL, 1.0~1.5 mM / L ATP, 1.0~1.5 mM / L DTT, 1.0~1.5 mM / L MgCl2, 15~20 mM / L CaCl2, and the pH of the buffer solution is 7.0~8.0; S2. Synthesis of nanofibrous silica under the guidance of fibrous actin: Add 0.1-0.2 volume of tetraethyl orthosilicate to the fibrous actin solution in step S1, adjust the pH of the solution, mineralize at room temperature, and obtain fibrous silica by freeze-drying.

2. The method for preparing nanofiber silica by actin biomineralization according to claim 1, characterized in that: In the step S1, the molecular weight of actin is 42-43 kDa.

3. The method for preparing nanofiber silica by actin biomineralization according to claim 2, characterized in that: In step S1, the actin concentration in the solution is 4-7 mg / mL.

4. The method for preparing nanofiber silica by actin biomineralization according to claim 3, characterized in that: In the step S1, the stirring time is 3 min, and the polymerization time at room temperature is 4 to 6 h.

5. The method for preparing nanofiber silica by actin biomineralization according to claim 1, characterized in that: In step S2, the concentration of tetraethyl orthosilicate is 0.75 M / L.

6. The method for preparing nanofiber silica by actin biomineralization according to claim 1, characterized in that: In step S2, the pH of the solution is adjusted to 4.0-9.0, the room temperature mineralization time is 5-7 days, and the freeze-drying time is 12-24 hours.

Citation Information

Patent Citations

  • Preparation method of laminated waterproof fabric

    CN109677094A

  • Preparation method of waterproof and moisture-permeable TPU hot melt adhesive film

    CN111300719A

  • Waterproof moisture-permeable terylene cotton cloth TPU composite fabric

    CN213920056U

  • Preparation method of biomimetic silica nanotubes

    CN105084371A

  • Hollow fibrous silica and its production