Biological repair material and its preparation method and application

By using crosslinking technology in biorepair materials to combine collagen with decellularized tissue membrane or electrospinned collagen membrane, the problems of poor bonding and poor degradation performance in the prior art are solved, and high viscosity, strength and Biocompatible biorepair material suitable for a variety of tissue repairs.

CN117462755BActive Publication Date: 2024-11-12BEIJING COMPONT MEDICAL DEVICES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311587461.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-24
Publication Date
2024-11-12
Estimated Expiration
2043-11-24

AI Technical Summary

Technical Problem

The existing self-adhesive repair materials have the risk of poor bonding and falling off during use, insufficient elasticity and toughness, and poor degradation performance of the membrane base material, which cannot be used for repair of multiple tissues.

Method used

Crosslinking technology is used to form a crosslinking structure between collagen as a bioadhesive layer and decellularized tissue membrane or electrospinned collagen membrane substrate to enhance adhesion and crosslinking through defoaming, irradiation and lyophilization treatment. Prepare biorepair materials to ensure the viscosity and strength of the materials in wet environments.

Benefits of technology

Improves the mechanical strength and biocompatibility of biorepair materials, controllable degradation performance, and is suitable for repair of a variety of tissues, including dura, oral cavity, abdominal wall, tendon, etc., reducing adhesion and secondary trauma, providing Good sealing effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117462755B_ABST
    Figure CN117462755B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of biomedicine and biomaterial technology, and discloses a biorepair material, a preparation method thereof, and an application thereof. The biorepair material comprises a substrate and a bioadhesive layer; the substrate and the bioadhesive layer are bonded by a cross-linked structure formed by radiation cross-linking. The method comprises: spreading a bioadhesive solution on a substrate, and sequentially performing defoaming treatment, radiation cross-linking treatment, and freeze-drying treatment to obtain the biorepair material. The components of the substrate and the bioadhesive layer in the biorepair material provided by the present invention both contain collagen, and the two are cross-linked by radiation using water molecules as a medium, so that the collagen molecules are cross-linked from the original linear macromolecules to three-dimensional network molecules, so that the substrate and the bioadhesive layer are chemically bonded, thereby increasing the mechanical strength of the two, and ensuring that there will be no undesirable phenomena such as loose adhesion and connection detachment during use and repair.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of biomedicine and biomaterials, and in particular to a biological repair material and a preparation method and application thereof. Background Art

[0002] Self-adhesive repair materials can eliminate the need for surgical sutures, greatly reducing operation time and lowering surgical operation risks.

[0003] Self-adhesive repair materials are generally divided into two structures: one is the self-adhesive part with adhesive effect, and the other is the membrane base material with shielding and repairing functions. Existing repair materials have the following problems: (1) The self-adhesive part and the membrane base material are mostly physically connected by the adhesive force of the self-adhesive part itself, which may cause the risk of falling off during use; (2) The self-adhesive part is a degradable polyester medical self-adhesive layer or α-cyanoacrylate butyl medical self-adhesive layer. This type of medical adhesive has strong adhesive force, but insufficient elasticity and toughness; (3) Existing membrane base materials are polymer synthetic materials or animal-derived materials, such as polylactic acid, polyglycolic acid, or bovine pericardial tissue, bovine tendon, porcine pericardium, etc. These membrane materials have poor degradation performance or no degradation performance; (4) Existing self-adhesive repair materials are mostly used for the repair of dura mater and cannot be used for the repair of multiple tissues. Summary of the invention

[0004] In order to solve one or more technical problems in the prior art, the present invention provides a biological repair material and a preparation method and application thereof.

[0005] In the biorepair material of the present invention, the adhesion between the substrate and the bioadhesive layer is strengthened by cross-linking, and the bioadhesive layer has high bonding properties, good biocompatibility, good elasticity and toughness, and can maintain viscosity and strength in a wet environment; the substrate has good mechanical properties, biocompatibility and degradation properties. The biorepair material of the present invention can be used to repair various tissues such as dura mater, oral cavity, abdominal wall, epidermis, tendon, etc.

[0006] In order to achieve the above-mentioned object, the first aspect of the present invention provides a biological repair material, which comprises a substrate and a biological adhesive layer; the substrate is a decellularized tissue membrane or an electrospun collagen membrane; the biological adhesive layer is made of a biological adhesive comprising collagen;

[0007] Wherein, the substrate and the bioadhesive layer are bonded via a cross-linked structure formed by radiation cross-linking.

[0008] The second aspect of the present invention provides a method for preparing the biorepair material described in the first aspect, the method comprising: spreading a bioadhesive solution on a substrate, and sequentially performing defoaming treatment, radiation cross-linking treatment and freeze-drying treatment to obtain the biorepair material.

[0009] The third aspect of the present invention provides a biological repair material obtained by the preparation method described in the second aspect.

[0010] The fourth aspect of the present invention provides use of the biological repair material described in the first aspect or the third aspect in tissue repair.

[0011] Through the above technical solution, the beneficial technical effects achieved by the present invention are as follows:

[0012] (1) The components of the base and the bioadhesive layer in the biorepair material provided by the present invention both contain collagen, and the collagen molecules are cross-linked by radiation using water molecules as a medium, thereby cross-linking the original linear macromolecules into three-dimensional network molecules, so that the base and the bioadhesive layer are chemically bonded, thereby increasing the mechanical strength of the two, ensuring that undesirable phenomena such as weak adhesion and connection detachment will not occur during use and repair;

[0013] (2) The substrate and bioadhesive layer in the biorepair material provided by the present invention are both made of fully absorbable materials, which have good biocompatibility; the substrate is a decellularized tissue membrane or an electrospun collagen membrane, which has its own gaps, facilitating rapid cell growth and facilitating tissue repair; the bioadhesive layer can assist in fixing the substrate, avoiding secondary trauma caused by the fixing process, and can provide a sealing effect, making the biorepair material of the present invention particularly suitable for sealing wounds and incisions with fluid or gas leakage;

[0014] (3) The degradation cycle of the biorepair material of the present invention is controllable, and different products can be designed for use in different locations and indications. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 is a schematic diagram of the structure of the biological repair material of the present invention;

[0016] Figure 2 This is a 4.5x electron microscope image of the biological repair material prepared in Example 1 of the present invention;

[0017] Figure 3 This is a front view of the biological repair material product prepared in Example 1 of the present invention;

[0018] Figure 4 This is a back view of the biological repair material product prepared in Example 1 of the present invention;

[0019] Figure 5This is the test diagram of the tensile testing machine;

[0020] Figure 6 It is a schematic diagram of a trapezoidal template.

[0021] Wherein: 1-substrate; 2-cross-linking structure; 3-bioadhesive layer. DETAILED DESCRIPTION

[0022] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0023] The first aspect of the present invention provides a biological repair material, which comprises a substrate and a biological adhesive layer; the substrate is a decellularized tissue membrane or an electrospun collagen membrane; the biological adhesive layer is made of a biological adhesive comprising collagen;

[0024] Wherein, the substrate and the bioadhesive layer are bonded via a cross-linked structure formed by radiation cross-linking.

[0025] The structure of the biorepair material of the present invention is as follows Figure 1 shown.

[0026] In some embodiments of the present invention, the decellularized tissue membrane is selected from one of decellularized porcine small intestinal submucosa, decellularized dermal matrix or decellularized pericardium.

[0027] The preparation process of the decellularized tissue membrane includes the steps of pretreatment, virus inactivation, decellularization, cleaning, and molding. The methods used in each step are all common methods in the prior art, and the decellularization step uses an acid-base method for decellularization. The specific method is: decellularize the virus-inactivated pig small intestinal submucosal matrix material using an acid solution or an alkaline solution in an ultrasonic cleaning machine.

[0028] The acid solution used can be one or more of hydrochloric acid, sulfuric acid, nitric acid, and formic acid. The concentration of the acid solution is 0.001-1 mol / L, the volume of the acid solution is 2-20 times the volume of the pretreated pig small intestine material, and the time for decellularization with the acid solution is 30-120 min; the alkaline solution can be KOH solution and / or NaOH solution, the concentration of the alkaline solution is 0.001-1 mol / L, the volume of the alkaline solution is 2-20 times the volume of the pretreated pig small intestine material, and the time for decellularization with the alkaline solution is 30-120 min.

[0029] The molding operation can be performed by drying molding or freeze-drying molding.

[0030] In some embodiments of the present invention, the electrospun collagen membrane is prepared by electrospinning a mixture of collagen fibers and L-arginine.

[0031] The preparation process includes preparing a collagen fiber solution, preparing an L-arginine solution, mixing the two solutions, and performing electrostatic spinning using an electrostatic spinning machine.

[0032] In some embodiments of the present invention, the bioadhesive layer is made of a bioadhesive comprising a supercharged protein and a surfactant; the surfactant is a cationic surfactant or an anionic azobenzene surfactant; and the cationic surfactant has a catechol structural unit.

[0033] In some embodiments of the present invention, the bioadhesive is composed of a super positively charged protein and an anionic azobenzene surfactant; or, the bioadhesive is composed of a super negatively charged protein and a cationic surfactant.

[0034] In some embodiments of the present invention, the thickness of the substrate is 0.05-0.15 mm, and the thickness of the bioadhesive layer is 2-5 mm.

[0035] In some embodiments of the present invention, the thickness of the substrate is 0.16-0.25 mm, and the thickness of the bioadhesive layer is 6-10 mm.

[0036] In some embodiments of the present invention, the thickness of the substrate is 0.26-0.35 mm, and the thickness of the bioadhesive layer is 11-15 mm.

[0037] The above three combinations of thickness of the base and the bioadhesive layer represent three different types of biorepair materials, namely low type, medium type and high type.

[0038] The biological repair material described in the present invention can be used to repair various tissues such as dura mater, oral cavity, hernia defect, skin defect, tendon, etc. According to the needs of different tissues, different tissues can be repaired by using different types of repair materials. For example, low-type repair materials can be used for repairing dura mater or oral cavity, medium-type repair materials can be used for repairing hernia defect or skin defect, and high-type repair materials can be used for repairing tendons and other tissues.

[0039] The second aspect of the present invention provides a method for preparing the biorepair material described in the first aspect, the method comprising: spreading a bioadhesive solution on a substrate, and sequentially performing defoaming treatment, radiation cross-linking treatment and freeze-drying treatment to obtain the biorepair material.

[0040] The above preparation method can be carried out in a mold, such as a mold box with a certain height, length and width, and the material can be a polymer material such as organic glass, polytetrafluoroethylene, or a metal material such as stainless steel.

[0041] In some embodiments of the present invention, the defoaming treatment is performed by vibration defoaming or vacuum defoaming. The vibration defoaming can be performed by ultrasonic vibration, and the vacuum defoaming can be performed by a vacuum box. The vacuum degree during vacuum defoaming is -40 to -80 KPa. In the present invention, if the vacuum degree is too small, the defoaming effect cannot be achieved; if the vacuum degree is too large, the bioadhesive on the upper layer will overflow the mold.

[0042] In some embodiments of the present invention, 60Coγ rays are used for irradiation cross-linking.

[0043] In some embodiments of the present invention, the irradiation dose is 5-15 kGy.

[0044] In the present invention, the following scheme can be adopted for freeze drying: the freeze drying includes a pre-freezing stage, a first sublimation stage, a second sublimation stage and a cooling stage, and the process conditions of each stage are as follows:

[0045] Pre-freezing stage: target temperature is -20 to -15°C, rate is 3-4.0°C / min, constant temperature time is 160-240min;

[0046] The first sublimation stage: vacuuming, vacuum degree is lower than -0.05MPa, gas mixing 50-120Pa, including three temperature rising steps, namely:

[0047] -10 to -8°C, rate 0.2-0.3°C / min, constant temperature time 150-180min;

[0048] 1~2℃, rate is 0.1-0.2℃ / min, constant temperature time is 150-180min;

[0049] 4-10℃, rate is 0.3-0.4℃ / min, constant temperature time is 180-240min;

[0050] The second sublimation stage: vacuuming, vacuum degree is lower than -0.05MPa, gas mixing 50-120Pa, including four temperature rise steps, namely:

[0051] 14-20℃, rate is 1.0-1.2℃ / min, constant temperature time is 120-140min;

[0052] 22-32℃, rate is 1.0-1.2℃ / min, constant temperature time is 120-140min;

[0053] 34-38℃, rate is 1.6-1.8℃ / min, constant temperature time is 70-80min;

[0054] 42-45℃, rate is 1.6-1.8℃ / min, constant temperature time: endpoint judgment is carried out every 1 hour until the endpoint judgment is qualified; endpoint ≤0.5Pa / 10min;

[0055] Cooling stage: cool to room temperature at a rate of 4-6℃ / min.

[0056] The third aspect of the present invention provides a biological repair material obtained by the preparation method described in the second aspect.

[0057] The fourth aspect of the present invention provides use of the biological repair material described in the first aspect or the third aspect in tissue repair.

[0058] In some embodiments of the invention, the tissue is dura mater, oral cavity, abdominal wall, extraperitoneal hernia, skin or tendon.

[0059] According to a particularly preferred embodiment of the present invention, a method for preparing a self-adhesive biological repair material comprises the preparation of a biological adhesive, the preparation of a decellularized porcine small intestinal submucosal matrix, and the preparation of a self-adhesive biological repair material, wherein the method comprises the following steps:

[0060] (1) Transform the super positively charged protein K series or super negatively charged protein E series vector plasmids into Escherichia coli expression strains (BL21 / BL21DE3 / BLRD E3) for overexpression. Collect the cells after induction for 12 hours, resuspend them in lysis buffer, add protease inhibitors, DNA enzyme, and lysozyme, crush the cells with a high-pressure crusher, centrifuge at a speed of more than 10,000 rpm, collect the supernatant, and purify it by HPLC to finally obtain super positively charged protein K or super negatively charged protein E;

[0061] (2) adding the surfactant solution dropwise to the super-charged protein solution and mixing them evenly to obtain an adhesive solution; wherein the super-positively charged protein K needs to be mixed with an anionic azobenzene surfactant, and the super-negatively charged protein E needs to be mixed with a cationic surfactant;

[0062] (3) taking the pig small intestine submucosa material, removing the surface fat and lymphatic tissue, and washing it with an ultrasonic cleaning machine to obtain a pretreated submucosa raw material;

[0063] (4) soaking the pretreated pig small intestinal submucosal material obtained in step (3) in a "peracetic acid-ethanol" solution in an ultrasonic cleaning machine, and then washing it with purified water to obtain a virus-inactivated submucosal material;

[0064] (5) decellularizing the virus-inactivated submucosal material obtained in step (4) using an acid solution or an alkaline solution in an ultrasonic cleaning machine; repeating this step 1-5 times (e.g., 1, 2, 3, 4 or 5 times) after replacing the solution to obtain a decellularized material;

[0065] (6) fixing the decellularized porcine small intestinal submucosa matrix material obtained in step (5) onto a mold, and drying or freeze-drying the material to obtain a decellularized porcine small intestinal submucosa matrix;

[0066] (7) selecting a corresponding mold box, spreading the decellularized porcine small intestinal submucosal matrix obtained in step (6) on the bottom of the mold, measuring a certain amount of the adhesive solution obtained in step (2), injecting it into the mold and shaking it evenly to keep the liquid surface flat;

[0067] (8) Place the injected mold in an ultrasonic device or vacuum box to eliminate bubbles in the liquid in the mold and measure the product thickness;

[0068] (9) subjecting the defoamed material to irradiation cross-linking treatment, with the irradiation dose being 5-15 KGy;

[0069] (10) The radiation-crosslinked material is placed in a freeze dryer for freeze drying to obtain an absorbable biorepair material with a self-adhesive structure.

[0070] The present invention will be described in detail below through examples.

[0071] In the following examples and comparative examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if no manufacturer is specified, are all conventional products that can be obtained through commercial channels.

[0072] Example 1

[0073] This example is used to illustrate the preparation of biological repair materials.

[0074] (1) Transforming the super positively charged protein K series vector plasmids into the Escherichia coli expression strain, collecting the cells after expression induction for 12 hours, resuspending, breaking, centrifuging, collecting the supernatant, and purifying to obtain the super positively charged protein K;

[0075] (2) adding the anionic azobenzene surfactant solution dropwise to the super charged protein K solution and mixing well to obtain an adhesive solution;

[0076] (3) taking the pig small intestine submucosa material, removing the surface fat and lymphatic tissue, and washing it with an ultrasonic cleaning machine to obtain a pretreated submucosa raw material;

[0077] (4) soaking the pretreated porcine small intestinal submucosal material obtained in step (3) in a "peracetic acid-ethanol" solution in an ultrasonic cleaning machine, and then washing it with purified water to obtain a virus-inactivated submucosal material, wherein the "peracetic acid-ethanol" solution has a composition of peracetic acid: ethanol: water = 1:24:75, the ultrasonic cleaning machine frequency is 40 kHz, and the treatment time is 60 min;

[0078] (5) decellularizing the virus-inactivated submucosal material obtained in step (4) using an acid solution in an ultrasonic cleaning machine; the acid solution is hydrochloric acid with a concentration of 0.5 mol / L, the volume of hydrochloric acid used is 10 times that of the material obtained in step (4), the frequency of the ultrasonic cleaning machine is 25 kHz, and the time for decellularization using the acid solution is 60 min;

[0079] (6) fixing the decellularized porcine small intestinal submucosa matrix material obtained in step (5) onto a mold and freeze-drying the material to obtain a decellularized porcine small intestinal submucosa matrix having a thickness of 0.15 mm;

[0080] (7) Select a mold box with a size of 15 cm × 10 cm × 2.5 cm, cut the decellularized porcine small intestinal submucosal matrix obtained in step (6) into 15 cm × 10 cm, spread it on the bottom of the mold, and then inject the adhesive solution obtained in step (2) into the mold. The injection height of the solution is 4 mm, and shake it evenly to keep the liquid surface as flat as possible;

[0081] (8) Place the injected mold in a vacuum box to eliminate bubbles in the liquid in the mold;

[0082] (9) The defoamed material is subjected to irradiation cross-linking treatment using 60Co γ-rays, and the irradiation dose is selected to be 5 kGy;

[0083] (10) After the irradiation cross-linking treatment, the material is placed in a freeze dryer for freeze drying to obtain an absorbable biological repair material with a self-adhesive structure. This material can be used to repair the oral cavity and dura mater.

[0084] Figure 2 This is a 4.5x electron microscope image of the biological repair material;

[0085] Figure 3 is a front view of the biological repair material product;

[0086] Figure 4 is a back view of the biological repair material product;

[0087] Example 2

[0088] This example is used to illustrate the preparation of biological repair materials.

[0089] (1) Transforming the super negatively charged protein E series vector plasmids into the Escherichia coli expression strain, collecting the bacteria after expression induction for 12 hours, resuspending, breaking, centrifuging, collecting the supernatant, and purifying to obtain the super positively charged protein E;

[0090] (2) adding a cationic surfactant solution having a catechol structural unit dropwise to the super charged protein E solution and mixing well to obtain an adhesive solution;

[0091] (3) taking the pig small intestine submucosa material, removing the surface fat and lymphatic tissue, and washing it with an ultrasonic cleaning machine to obtain a pretreated submucosa raw material;

[0092] (4) soaking the pretreated porcine small intestinal submucosal material obtained in step (3) in a "peracetic acid-ethanol" solution in an ultrasonic cleaning machine, and then washing it with purified water to obtain a virus-inactivated submucosal material, wherein the "peracetic acid-ethanol" solution has a composition of peracetic acid: ethanol: water = 1:24:75, the ultrasonic cleaning machine frequency is 40 kHz, and the treatment time is 60 min;

[0093] (5) decellularizing the virus-inactivated submucosal material obtained in step (4) using an alkaline solution in an ultrasonic cleaning machine; the alkaline solution is a NaOH solution with a concentration of 0.5 mol / L, the volume of NaOH used is 5 times that of the material obtained in step (4), the frequency of the ultrasonic cleaning machine is 25 kHz, and the decellularization time using the alkaline solution is 60 min;

[0094] (6) fixing the decellularized porcine small intestinal submucosa matrix material obtained in step (5) onto a mold and freeze-drying the material to obtain a decellularized porcine small intestinal submucosa matrix having a thickness of 0.25 mm;

[0095] (7) Select a mold box with a size of 15 cm × 10 cm × 2.5 cm, cut the decellularized porcine small intestinal submucosal matrix obtained in step (6) into 15 cm × 10 cm, spread it on the bottom of the mold, and then inject the adhesive solution obtained in step (2) into the mold. The injection height of the solution is 12 mm, and shake it evenly to keep the liquid surface as flat as possible;

[0096] (8) Place the injected mold in a vacuum box to eliminate bubbles in the liquid in the mold;

[0097] (9) The defoamed material is subjected to irradiation cross-linking treatment using 60Coγ-rays, with an irradiation dose of 10 kGy;

[0098] (10) The cross-linked material is placed in a freeze dryer for freeze drying to obtain an absorbable biological repair material with a self-adhesive structure. This material can be used to repair tendons.

[0099] Example 3

[0100] This example is used to illustrate the preparation of biological repair materials.

[0101] (1) Transforming the super positively charged protein K series vector plasmids into the Escherichia coli expression strain, collecting the cells after expression induction for 12 hours, resuspending, breaking, centrifuging, collecting the supernatant, and purifying to obtain the super positively charged protein K;

[0102] (2) adding the anionic azobenzene surfactant solution dropwise to the super charged protein K solution and mixing well to obtain an adhesive solution;

[0103] (3) Under the action of magnetic stirring, collagen was dissolved in an acetic acid solution (acetic acid concentration was 25 wt%) to prepare a 1 wt% collagen fiber solution, which was solution 1; L-arginine hydrochloride was dissolved in an acetic acid solution (acetic acid concentration was 20 wt%) to prepare a 7 wt% L-arginine solution, which was solution 2;

[0104] (4) Solution 1 and solution 2 were mixed in a mass ratio of 9:1 and subjected to electrospinning. The electrospinning parameters were set as follows: electrospinning distance 15 cm, electrospinning voltage 15 kV, solution flow rate 2 mL / h, receiving device rotation rate 500 rpm, and syringe lateral movement speed 10 cm / min; the collagen fiber membrane was collected on a flat aluminum foil receiving device; the obtained nanofiber membrane was vacuum dried for 24 h to obtain an electrospun collagen membrane with a thickness of 0.2 mm;

[0105] (5) Select a mold box with a size of 15 cm × 10 cm × 2.5 cm, cut the electrospun collagen membrane obtained in step (4) into 15 cm × 10 cm, spread it on the bottom of the mold, and then inject the adhesive solution obtained in step (2) into the mold. The injection height of the solution is 4 mm, shake it evenly, and try to keep the liquid surface flat;

[0106] (6) Place the injected mold in a vacuum box to eliminate bubbles in the liquid in the mold;

[0107] (7) The defoamed material is subjected to irradiation cross-linking treatment using 60Co γ-rays, and the irradiation dose is selected to be 5 kGy;

[0108] (8) After the irradiation cross-linking treatment, the material is placed in a freeze dryer for freeze drying to obtain an absorbable biological repair material with a self-adhesive structure. This material can be used to repair the oral cavity and dura mater.

[0109] Comparative Example 1

[0110] The self-adhesive dura mater patch prepared in Example 2 of CN108272529A was used as Comparative Example 1.

[0111] Test Example 1 Breaking Strength and Tensile Strength Test

[0112] According to the standard method of GB / T 3923.1-2013, the materials of Examples 1, 2 and Comparative Example 1 were trimmed into rectangular specimens of 150 mm × 50 mm, and the specimens were placed on a testing machine for tensile strength testing. The experimental conditions were: gauge length of 100 mm, tensile speed of 50 mm / min, and pretension of 2 N. Figure 5 shown.

[0113] The results are shown in Table 1.

[0114] Table 1

[0115] project Breaking strength / N Tensile strength / N / cm Elongation at break / % Example 1 224.3 44.86 34.45 Example 2 563.2 82.3 58.6 Comparative Example 1 58.6 11.72 18.63

[0116] It can be seen from the results in Table 1 that the biological repair materials prepared in Examples 1 and 2 have significantly improved tensile strength and elongation at break compared with existing materials, and can meet the clinical needs of repair materials.

[0117] Test Example 2 Tear Strength Test

[0118] According to the method specified in GB / T 3917.3-2009, the materials of Examples 1, 2 and Comparative Example 1 were cut into rectangular specimens of 150 mm × 75 mm, and the samples were cut into rectangular specimens according to the trapezoidal sample diagram (such as Figure 6 The samples were cut into pieces (as shown in the figure), and the samples were placed on a testing machine for tear strength test. The experimental conditions were: the gauge length was 25 mm, and the tensile speed was 100 mm / min.

[0119] The results are shown in Table 2.

[0120] Table 2

[0121] project Tear strength / N Example 1 107.3 Example 2 246.1 Comparative Example 1 36.2

[0122] It can be seen from the test results in Table 2 that the tear strength of the materials prepared in Examples 1 and 2 is greatly improved compared with the existing materials.

[0123] Test Example 3 Peel Strength Test

[0124] According to the standard method of GB / T 2791-1995, a "T"-shaped open specimen was prepared. The total length of the specimen was 200 mm, the length of the bonding part was 150 mm, and the width of the specimen was 25 mm. The specimen was placed on a testing machine for tear strength test. The experimental conditions were: the tensile speed was 100 mm / min.

[0125] The results are shown in Table 3.

[0126] Table 3

[0127] project Peel force / N Peel strength / N / cm Example 1 15.6 6.24 Example 2 16.9 7.02 Comparative Example 1 8.5 3.40

[0128] From the test results in Table 3, it can be seen that the materials prepared in Examples 1 and 2 significantly increase the connection strength between the bioadhesive layer and the basement membrane material through radiation cross-linking, and the peeling force and peeling strength are significantly improved compared with the existing materials.

[0129] From the above results, it can be seen that the connection between the self-adhesive layer and the film base material in Comparative Example 1 is only based on the physical viscosity of the self-adhesive itself, and there is a risk of cracking and falling off during use. The bioadhesive layer and the base material of the present invention are cross-linked by radiation to form a three-dimensional network structure, which greatly enhances the connection strength between the two. A conclusion can be drawn from the comparative test of peel force and peel strength.

[0130] The pressure-sensitive adhesive of the self-adhesive layer in Comparative Example 1 is a non-absorbable material, while the bioadhesive used in the present invention can be degraded in vivo and has good biocompatibility.

[0131] The membrane base material in Comparative Example 1 is collagen sponge. The thickness of 5 mm of the collagen sponge is too large to be conducive to surgical operation, and the mechanical properties of the sponge are poor. The membrane base material of the present invention is a multilayer decellularized matrix or an electrospun polymer absorbable material, which has good mechanical properties. The breaking strength, tensile strength, tear strength and other properties are all better than those of Comparative Example 1. Conclusions can be drawn from relevant comparative tests.

[0132] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A biological repair material, characterized in that: The biological repair material comprises a substrate and a biological adhesive layer; the substrate is a decellularized tissue membrane obtained after decellularization and freeze-drying; the biological adhesive layer is made of a biological adhesive including collagen; Wherein, the substrate and the bioadhesive layer are bonded to each other by a cross-linked structure formed by irradiation cross-linking using 60Coγ rays; The acellular tissue membrane is selected from one of acellular porcine small intestinal submucosa, acellular dermal matrix or acellular pericardium; The bioadhesive is composed of a super positively charged protein and an anionic azobenzene surfactant; or, the bioadhesive is composed of a super negatively charged protein and a cationic surfactant, wherein the cationic surfactant has a catechol structural unit; The preparation method of the biological repair material comprises the following steps: (1) preparing a decellularized tissue membrane obtained after decellularization and freeze-drying as a substrate; (2) spreading the bioadhesive solution on a substrate, and sequentially performing defoaming treatment, radiation cross-linking treatment, and freeze-drying treatment to obtain the biorepair material; Among them, 60Coγ rays are used for irradiation cross-linking treatment.

2. The biorepair material according to claim 1, wherein: The thickness of the substrate is 0.05 mm-0.15 mm, and the thickness of the bioadhesive layer is 2 mm-5 mm.

3. A method for preparing a biological repair material according to claim 1 or 2, characterized in that: The method comprises the following steps: (1) preparing a decellularized tissue membrane obtained after decellularization and freeze-drying as a substrate; (2) spreading the bioadhesive solution on a substrate, and sequentially performing defoaming treatment, radiation cross-linking treatment, and freeze-drying treatment to obtain the biorepair material; Among them, 60Coγ rays are used for irradiation cross-linking treatment.

4. The preparation method according to claim 3, wherein The defoaming treatment method is vibration defoaming or vacuum defoaming.

5. The preparation method according to claim 4, wherein: The vacuum degree during vacuum defoaming is -40 to -80 KPa.

6. The preparation method according to claim 3, wherein: The irradiation dose is 5-15 kGy.

7. A biological repair material obtained by the preparation method according to any one of claims 3 to 6.

8. Use of the biological repair material according to any one of claims 1 to 2 or 7 in the preparation of tissue repair materials.

9. The use according to claim 8, wherein: The tissue is dura mater, oral cavity, abdominal wall, extraperitoneal hernia, skin or tendon.