A process for extracting lithium from waste battery black powder by roasting and leaching
Through the combined process of roasting and acid leaching, the problems of low lithium recovery rate and high lithium extraction cost in waste batteries are solved, efficient lithium recycling and low-cost production are achieved, ammonia is avoided, and lithium battery powder is ensured. High quality recycling.
Patent Information
- Application Number
- CN202311819249.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-27
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-12-27
AI Technical Summary
In the prior art, the lithium recovery rate in waste battery black powder is low, the lithium extraction cost is high, and there is a problem of ammonia gas generation. The lithium extraction method of lithium battery powder cannot guarantee the efficient recovery rate of lithium.
Using a combination of roasting and acid leaching, the baking temperature and acidity are controlled through the steps of two-stage roasting, acid leaching, impurity removal, ion exchange, lithium precipitation, washing, drying, crushing, demagnetization, mixing and packaging, and the baking temperature and acidity are increased. Lithium recovery rate reduces costs and avoids ammonia production.
It improves the recovery rate of lithium in waste batteries, reduces the cost of lithium extraction, avoids the production of ammonia, ensures the quality of lithium carbonate, and enhances the efficiency of lithium recycling and product quality.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium battery material recovery and relates to a process for extracting lithium from black powder of waste batteries by roasting and leaching. Background Art
[0002] Waste battery black powder is generally divided into ternary battery powder, iron-lithium battery powder and iron-lithium pole piece powder, etc. Among them, ternary battery black powder contains a large amount of metals such as cobalt, nickel, lithium and copper. Most manufacturers use nickel, cobalt and copper to extract lithium first, and the recovery rate of lithium extraction by this method is generally low; some companies use lithium extraction first and then other valuable metals. In this method, if nickel, cobalt, copper and other metals are leached in large quantities in the leaching section, the cost of lithium carbonate per ton is relatively high. There are two methods for extracting lithium from waste battery powder by roasting in China: Publication No. CN111893319A introduces a method for extracting lithium from waste batteries. This method uses ammonium sulfate and battery powder mixed with acid for a first-stage roasting treatment. During the process, a large amount of ammonia will be generated and needs to be treated; Publication No. CN106848473A introduces a selective recovery of lithium from waste lithium iron phosphate batteries. This method uses a direct high-temperature roasting of lithium waste iron lithium powder, and the total recovery rate of lithium cannot be guaranteed. Summary of the invention
[0003] In order to solve the problems existing in the prior art, the present invention adopts the following technical solutions:
[0004] The invention provides a process for extracting lithium from waste battery black powder by roasting and leaching. The process is characterized in that waste battery black powder is used as raw material, a roasting and acid leaching method is adopted, and the process comprises two-stage roasting, acid leaching, one-stage impurity removal, two-stage impurity removal, ion exchange, lithium precipitation, washing, drying, crushing, demagnetization, mixing and packaging to obtain battery-grade lithium carbonate.
[0005] Furthermore, the process adopts a method of roasting first and then leaching, and is carried out according to the following steps:
[0006] (1) Use an externally heated rotary kiln to complete the two-stage roasting of waste battery black powder. The main purpose of the first stage roasting is to destroy organic matter, and the main purpose of the second stage roasting is to make lithium exist in the form of lithium oxide.
[0007] (2) The acid leaching is carried out by controlling the residual acidity in the liquid after the reaction to be 4.0-7.0%, thereby ensuring that the lithium content of the leached slag is less than 0.10%.
[0008] (3) Remove the main impurities through neutralization reaction, and then use ion exchange to complete the lithium sulfate refining process, precipitate lithium to obtain lithium carbonate products, use centrifuge for deep washing, dryer to remove moisture, air flow milling to meet the product particle size requirements, and use mixing equipment, demagnetizer and baler to complete the packaging of lithium carbonate products.
[0009] Furthermore, in step (1) and step (2), acid activation + two-stage high-temperature roasting + acid leaching are used for ternary battery powder; and one-stage low-temperature roasting + one-stage high-temperature roasting + acid leaching are used for iron-lithium electrode powder or iron-lithium battery powder.
[0010] Furthermore, in step (1), in order to increase the lithium oxide content, three sets of air blowing systems are added before, during and after the rotary kiln to ensure sufficient oxygen, which has a relatively low cost compared to direct oxygen blowing.
[0011] Furthermore, step (2) is to control the leaching of nickel, cobalt and manganese by controlling the ratio of liquid alkali to sulfuric acid for ternary battery powder, and leaching is performed using 70% sulfuric acid and 32% liquid alkali, and the residual acidity is within the range of 4-5% to complete the leaching.
[0012] Furthermore, step (2) is to leach the iron-lithium battery powder or the iron-lithium pole piece powder using sulfuric acid with a concentration of 70%, and the residual acidity is controlled at 5-7%.
[0013] Furthermore, step (2) is to control the leaching temperature at 80-85° C. by using a cooling water coil built into the leaching pot, and to use a Roots blower to blow air into the leaching pot to ensure the lithium leaching rate and reaction rate.
[0014] Furthermore, step (3) is to first use belt filtration to perform preliminary solid-liquid separation and washing on the lithium carbonate slurry, stir and wash it in a mixing barrel, and then use a centrifuge to perform deep washing. During the whole process, water is a countercurrent washing process, and after washing, it is sent to prepare sodium carbonate solution.
[0015] Furthermore, step (3) is to use microwave drying to dry the lithium carbonate product, and the moisture content after drying is ≤0.20%.
[0016] Furthermore, in step (3), all lithium carbonate slurry material outlets are designed with demagnetizers.
[0017] Beneficial effects: The present invention uses acid activation + two-stage high-temperature roasting + low-acid leaching to extract lithium to treat waste ternary battery powder, which improves lithium recovery rate, avoids ammonia generation, and reduces lithium extraction costs; for iron-lithium battery powder and pole piece powder, we use one-stage low-temperature roasting + one-stage high-temperature roasting + low-acid leaching to improve lithium recovery rate, reduce costs, and avoid the impact of organic matter on the quality of lithium carbonate. . DETAILED DESCRIPTION
[0018] The specific technical scheme of the present invention is further described in detail below in conjunction with the examples. The components involved in the examples are parts by mass or mass ratios, and the concentrations involved are all mass concentrations.
[0019] Technical solution 1: Use a mixer to mix ternary battery powder and concentrated sulfuric acid at high speed and then carry out two-stage high-temperature roasting, wherein the amount of concentrated sulfuric acid is 2.0-2.5 times the equivalent of the lithium content, the temperature is 500-550℃, the temperature of the rotary kiln slowly decreases from front to back, and the total roasting time is 2.0-3.0h. Subsequently, battery-grade lithium carbonate is obtained through acid leaching, one-stage impurity removal, two-stage impurity removal, ion exchange, lithium precipitation, drying, crushing, demagnetization, mixing and packaging. Example 1
[0020] Add a certain amount of ternary battery powder waste and 98% concentrated sulfuric acid into the mixing equipment for activation; use a shaftless screw to evenly transport it to the inside of the kiln, and control the temperature of the first stage at 550-520℃ and the temperature of the second stage at 520-500℃ by controlling the size of the valve; the calcined material is cooled in a cooling kiln and then enters the leaching pot through a weight-based silo; acid leaching conditions: 5T calcined ternary battery black powder, liquid-solid ratio of 2.5:1, temperature of 80-85℃, residual acidity of 4-5%, insulation time of 2h, and solid-liquid separation using a filter press to obtain a lithium solution containing 15-20g / l, and then go through the first stage of impurity removal, the second stage of impurity removal, ion exchange, lithium precipitation, drying, crushing, demagnetization, mixing and packaging to obtain battery-grade lithium carbonate.
[0021] The equipment that uses sulfuric acid and ternary powder to mix is a mortar mixer. Although it has a short service life, it has low cost and good mixing effect. The material state after mixing is slightly moist and has good dispersion.
[0022] Sulfuric acid is calculated based on 2.0 times the lithium content of one ton of ternary powder, and the mixing time is 1 hour.
[0023] After two stages of high-temperature roasting, the lithium content in the ternary battery slag is enriched to 1.2 times, which is beneficial to increase the lithium content in the solution after leaching and saves the concentration cost.
[0024] The qualified rate of the material after roasting is achieved by controlling the proportion of divalent iron in the total iron (in the range of 5%-10%), and can also be judged by the brick red color of the material after roasting.
[0025] In order to increase the oxidation rate of ferrous iron during roasting, three additional air blowing systems are added in the front, middle and rear of the rotary kiln.
[0026] The leaching stage controls the ratio of sulfuric acid to liquid alkali to control the excessive leaching of nickel, cobalt and manganese, thereby reducing the cost of subsequent impurity removal.
[0027] It is necessary to control the residual acidity of the liquid after the leaching reaction to 4-5% to ensure that the lithium content in the slag in the pot is ≤0.10%, so as to ensure that the leaching slag after the final washing is ≤0.15%.
[0028] The leached residue is washed by 2 countercurrent stirring washes and 1 flushing method. After washing, the average lithium content of the residue can be ≤0.15%.
[0029] The first stage of impurity removal slag is washed by 3 times of countercurrent stirring and 1 flushing. After washing, the average value of slag lithium can be ≤0.15%. Combined with the production data, the recovery rate of ternary battery powder is shown in Table 1.
[0030]
[0031] The bottom water used in the leaching pot comes from the water after leaching and a first stage of slag removal and washing, which further increases the lithium content in the leaching mother liquor.
[0032] The main impurity produced by the second stage impurity removal is calcium slag, which is used as an auxiliary material for the first stage impurity removal.
[0033] After ion exchange, the calcium ion requirement is ≤8mg / L to meet the quality requirements of refined lithium sulfate.
[0034] Microwave drying is used to remove moisture from lithium carbonate. After drying, the moisture content is ≤0.20%. Combined with production data, the quality of battery-grade lithium carbonate produced by ternary battery powder is shown in Table 2.
[0035]
[0036] Technical Solution 2: Use vacuum to transport lithium iron battery powder or pole piece powder into the rotary kiln, and directly carry out two-stage roasting, low temperature stage 300-350℃ roasting time 0.5-1h, high temperature stage 500-550℃ roasting time 0.5-1h; after roasting, the material is subjected to single acid leaching, first stage impurity removal, second stage impurity removal, ion exchange, lithium precipitation, drying, crushing, demagnetization, mixing and packaging to obtain battery-grade lithium carbonate. Example 2
[0037] The materials are directly added into the rotary kiln by vacuum conveying for two-stage roasting, with the low temperature stage at 300-350℃ and the roasting time at 0.5-1h, and the high temperature stage at 500-550℃ and the roasting time at 0.5-1h. After the roasted materials are cooled, they are temporarily stored in a weighing silo, and 4-5T of roasted iron-lithium battery powder / electrode powder are added into the leaching pot. According to the liquid-solid ratio of 2:1, the temperature is 70-75℃ and the reaction time is 2h, and a lithium solution containing 15-20g / l is obtained. Then, after the first stage of impurity removal, the second stage of impurity removal, ion exchange, lithium precipitation, drying, crushing, demagnetization, mixing and packaging, battery-grade lithium carbonate is obtained.
[0038] The powdered iron-lithium grade sheet powder / battery powder is transported to the inside of the rotary kiln by a vacuum conveying system, and the material roasting capacity is 1 ton / hour.
[0039] By controlling the kiln speed between 15-20HZ, it is ensured that the material has sufficient roasting time in the low temperature section and the high temperature section.
[0040] Since the lithium content in the iron-lithium powder raw material is relatively low compared to the ternary battery powder, the liquid-to-solid ratio in the leaching section is 2:1, and the liquid lithium content after leaching ranges from 15-20g / L.
[0041] The residual acidity of iron-lithium battery powder and electrode powder in the leaching pot needs to be controlled at 5-7%, which can ensure that the slag lithium in the leaching pot is ≤0.10%, and can ensure that the slag lithium after the final filter pressing and washing is ≤0.15%.
[0042] Since there are no impurity elements such as nickel, cobalt, and manganese in the iron lithium powder / electrode powder, there is no need to use alkali to suppress excessive leaching of other impurity elements.
[0043] The subsequent processing technology is the same as that of the above-mentioned scheme 1. Combined with the test data, the recovery rates of iron-lithium electrode powder and iron-lithium battery powder are shown in Table 3.
[0044]
[0045] Technical features not described in the present invention can be implemented by or using existing technologies, and will not be described in detail here. Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above implementation modes. Changes, modifications, additions or substitutions made by ordinary technicians in the field within the essential scope of the present invention should also fall within the protection scope of the present invention.
Claims
1. A process for extracting lithium from waste battery black powder by roasting and leaching, characterized in that: Using waste battery black powder as raw material, a method combining roasting and acid leaching is adopted, which includes two-stage roasting, acid leaching, one-stage impurity removal, two-stage impurity removal, ion exchange, lithium precipitation, washing, drying, crushing, demagnetization, mixing and packaging to obtain battery-grade lithium carbonate; the process adopts a roasting-then-leaching method, and is carried out according to the following steps: (1) Use an externally heated rotary kiln to complete the two-stage roasting of waste battery black powder. The main purpose of the first stage roasting is to destroy organic matter, and the main purpose of the second stage roasting is to make lithium exist in the form of lithium oxide; (2) The acid leaching is carried out by controlling the residual acidity in the liquid after the reaction to be 4.0-7.0%, thereby ensuring that the lithium content of the leached slag is less than 0.10%; (3) Remove the main impurities through neutralization reaction, and then use ion exchange to complete the lithium sulfate refining process, precipitate lithium to obtain lithium carbonate products, use a centrifuge to perform deep washing, use a dryer to remove moisture, and use air flow crushing to meet the product particle size requirements. The lithium carbonate products are packaged by a mixing device, a demagnetizer and a baler; wherein, in step (1) and step (2), for ternary battery powder, acid activation + two-stage high-temperature roasting + acid leaching are used, wherein the temperature of the first stage is 550-520°C and the temperature of the second stage is 520-500°C; for iron-lithium pole piece powder or iron-lithium battery powder, one-stage low-temperature roasting + one-stage high-temperature roasting + acid leaching are used, wherein the low-temperature stage is 300-350°C and the high-temperature stage is 500-550°C.
2. A process for extracting lithium from waste battery black powder by roasting and leaching according to claim 1, characterized in that: Step (1) is to increase the lithium oxide content by adding three sets of air blowing systems before, during and after the rotary kiln to ensure sufficient oxygen. The cost is relatively low compared to direct oxygen blowing.
3. A process for extracting lithium from waste battery black powder by roasting and leaching according to claim 1, characterized in that: Step (2) is to control the leaching of nickel, cobalt and manganese by controlling the ratio of liquid alkali to sulfuric acid for ternary battery powder. 70% sulfuric acid and 32% liquid alkali are used for leaching, and the residual acidity is within the range of 4-5% to complete the leaching.
4. A process for extracting lithium from waste battery black powder by roasting and leaching according to claim 1, characterized in that: Step (2) is to use sulfuric acid with a concentration of 70% to leach the iron-lithium battery powder or the iron-lithium pole piece powder, and the residual acidity is controlled at 5-7%.
5. The process for extracting lithium from waste battery black powder by roasting and leaching according to claim 1, characterized in that: Step (2) is to control the leaching temperature at 80-85° C. by using a cooling water coil built into the leaching pot, and to use a Roots blower to blow air into the leaching pot to ensure the lithium leaching rate and reaction rate.
6. A process for extracting lithium from waste battery black powder by roasting and leaching according to claim 1, characterized in that: Step (3) is to first use belt filtration to perform preliminary solid-liquid separation and washing on the lithium carbonate slurry, stir and wash it in a mixing barrel, and then use a centrifuge to perform deep washing. During the whole process, water is a countercurrent washing process, and after washing, it is sent to prepare sodium carbonate solution.
7. A process for extracting lithium from waste battery black powder by roasting and leaching according to claim 1, characterized in that: Step (3) is to use microwave drying to dry the lithium carbonate product, and the moisture content after drying is ≤0.20%.
8. A process for extracting lithium from waste battery black powder by roasting and leaching according to claim 1, characterized in that: Step (3) is that all lithium carbonate slurry material outlets are designed with demagnetizers.
Citation Information
Patent Citations
Selective recovery method of lithium in waste and old lithium iron phosphate batteries
CN106848473A
Method for extracting lithium from waste battery powder
CN111893319A
Comprehensive utilization method of lithium iron phosphate battery waste positive electrode powder
CN111206161A
Method for efficiently recycling ternary positive electrode material of waste lithium ion batteries
CN111733326A
Waste lithium ion battery recovery method
CN114085997A