A method for recycling secondary brand BPA through pretreatment and productization

The secondary BPA produced in phosgeneization method is processed through drying, dissolution, filtration and distillation steps, which solves the problems of low purity and many impurities, and realizes the recycling of high-purity BPA, avoiding resource waste and carbon dioxide emissions. Improve economic benefits and resource utilization.

CN117510309BActive Publication Date: 2024-12-03WANHUA CHEM GRP CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202210899976.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-28
Publication Date
2024-12-03
Estimated Expiration
2042-07-28

AI Technical Summary

Technical Problem

The secondary BPA produced in the PC production process of phosgeneization method cannot meet the national standard requirements due to its low purity and high impurity content, which can only be treated as solid waste and fail to effectively recycle and utilize resources.

Method used

A product recycling method for pretreatment of secondary BPA, including drying, dissolving, filtration and distillation steps: remove moisture through a dryer, add solvent to the dissolution tank to dissolve BPA, and remove the primary filter and the secondary filter respectively. Solid particles and trace impurities are recovered from the distillation tower to obtain a high-purity BPA product.

Benefits of technology

The purity of sub-brand BPA is improved, the production needs of high-purity BPA products are met, resource waste and carbon dioxide emissions are avoided, and the productive recycling of sub-brand BPA is realized, with great economic benefits and resource utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117510309B_ABST
    Figure CN117510309B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for pre-processing and productizing secondary brand BPA, comprising the following steps: 1) secondary brand BPA enters a paddle dryer to remove water, and controls the water content to be less than 50ppm; 2) adopts a solvent to dissolve into a BPA solution; 3) the BPA solution is subjected to two-stage filtration, the first-stage filtration removes large particles of sodium chloride, ferric chloride and PC solids, and the second-stage filtration adopts nanofiltration to deeply remove small particles of solid particles; 4) the BPA solution is subjected to rectification to recover the solvent, and obtain a high-purity BPA product. The method of the present invention adopts a brand-new nanofiltration membrane to effectively remove small particles and color-developing substances, and obtains a high-purity BPA product, wherein the BPA purity is 99.9% and the platinum-cobalt color number is not greater than 5.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of BPA preparation and relates to a method for recovering secondary brand BPA through pretreatment and productization. Background Art

[0002] Bisphenol A (BPA) is an important chemical raw material, mainly used to make polycarbonate and epoxy resin. Polycarbonate has high requirements for raw materials, requiring a purity of more than 99.85% and a platinum cobalt color number of less than 5. BPA is synthesized by alkylation reaction with phenol and acetone as raw materials, and purified by crystallization process to obtain a high-purity product that meets the needs of polycarbonate products.

[0003] Patent CN205914032 U discloses a micro-nano filtration membrane, which uses a polyamide and cellulose acetate composite membrane as a filtration layer for wastewater treatment to separate organic matter and salts. The composite membrane material has poor tolerance to organic substances such as isopropyl ether and BPA and cannot be used in the BPA system.

[0004] In the wastewater produced by the phosgenation process of PC, 1000ppm-8000ppm of BPA will remain. In the wastewater treatment unit, hydrochloric acid is added to the wastewater to adjust the pH to 1-6, and BPA is precipitated. The secondary brand BPA is obtained by drum filtration or column filtration. The waste BPA cannot meet the national product standards and can only be treated as solid waste. The currently disclosed patents do not involve the recovery process of the secondary brand BPA. Summary of the invention

[0005] During the research process on secondary brand BPA, the inventor found that secondary brand BPA mainly contains water, sodium chloride, ferric chloride, and PC. The presence of water will not only reduce the purity of BPA, but also affect the transportation of BPA solids. The presence of sodium chloride will affect the quality of PC after reuse. The purity of ferric chloride will affect the color number of BPA and then affect the background color of PC after reuse. Therefore, how to completely remove water, sodium chloride, ferric chloride, and PC from secondary brand BPA is the key to improving the purity of the product and reuse it for PC production. Based on this research, the present invention was completed.

[0006] The purpose of the present invention is to provide a method for pre-processing and productizing the recovery of secondary brand BPA in view of the problem that secondary brand BPA produced as a by-product in the existing phosgenation process for producing PC cannot meet the national standards due to its low purity and high impurity content, which can solve the problem that the secondary brand BPA has low purity and can only be used as solid waste.

[0007] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solution:

[0008] A method for recycling secondary brand BPA by pretreatment and productization, comprising the following steps:

[0009] 1) Wastewater containing secondary brand BPA from phosgenation PC enters the dryer to remove moisture;

[0010] 2) The secondary brand BPA treated in step 1) is placed in a dissolving tank with stirring, and a solvent is added to dissolve it to obtain a BPA solution;

[0011] 3) The BPA solution obtained in step 2) enters a primary filter to remove solid particles larger than 20 μm;

[0012] 4) The BPA solution after the treatment in step 3) enters a secondary filter to further remove solid particles;

[0013] 5) The BPA solution after the treatment in step 4) enters a distillation tower to remove and recover the solvent to obtain a high-purity BPA product.

[0014] In a specific embodiment, the secondary brand BPA in step 1) contains, based on total mass, 8-20% water, 1-2% sodium chloride, 10-100 ppm ferric chloride, 1000-3000 ppm PC, and 78%-90% BPA.

[0015] In a specific embodiment, in step 1), a high temperature gas is introduced as a carrier gas, and the temperature of the high temperature gas is 100-140° C., preferably 110-120° C.;

[0016] Preferably, the amount of the high temperature gas and the secondary brand BPA is 0.1-1Nm 3 / kg, preferably 0.5-0.8Nm 3 / kg;

[0017] Preferably, the high temperature gas is selected from hot air or hot nitrogen, preferably hot nitrogen;

[0018] Preferably, the dryer is selected from any one of a paddle dryer, a tube dryer, and a fluidized bed dryer, and preferably a paddle dryer;

[0019] Preferably, in step 1), the drying temperature is 100-140° C., preferably 110-120° C., and the residence time is 0.1-5 h, preferably 0.3-1 h.

[0020] In a specific embodiment, the solvent in step 2) is selected from at least one of methanol, ethanol, butanol, phenol, acetone, MTBE, and isopropyl ether, preferably isopropyl ether;

[0021] Preferably, the mass concentration of BPA in the prepared solution is 10%-30%, preferably 20%-25%.

[0022] In a specific embodiment, the primary filter in step 3) is a filter bag or a filter stick, preferably a filter stick;

[0023] Preferably, the filter rod material is selected from any one of 316L, polyphenylene sulfide, and PTFE, preferably polyphenylene sulfide.

[0024] In a specific embodiment, the filtration accuracy in step 3) is 10-50 μm, preferably 20-30 μm.

[0025] In a specific embodiment, the secondary filter in step 4) comprises a nanofiltration membrane;

[0026] Preferably, the nanofiltration membrane has a three-layer structure, the bottom layer is a support layer made of PTFE material, the middle layer is a filter layer made of PVDF material, and the top layer is a protective layer made of PP material;

[0027] More preferably, the support layer has a thickness of 2-3 mm and a pore size of 40-50 microns; the filter layer has a thickness of 2-3 mm and a pore size of 20-30 nanometers; and the protective layer has a thickness of 1-2 mm and a pore size of 10-20 microns.

[0028] In a specific embodiment, the distillation tower in step 5) is selected from any one of a plate tower, a structured packing tower, and a random packing tower, preferably a plate tower.

[0029] In a specific embodiment, the number of theoretical plates of the distillation tower is 20-35, the reflux ratio is 0.2-2, the bottom pressure is 10-30 kPa, and the bottom temperature is 190-210°C.

[0030] In a specific embodiment, the purity of the high-purity BPA product obtained in step 5) is greater than 99.9%, the platinum-cobalt color is not greater than 5, the sodium chloride is not greater than 0.01 ppm, the ferric chloride is less than 0.01 ppm, and the PC is less than 0.01 ppm.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] The only treatment method for secondary brand BPA in the prior art is incineration, which wastes resources and increases carbon dioxide emissions. The method of the present invention can convert secondary brand BPA into products, which has greater economic benefits and resource utilization. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a schematic diagram of the process of the preparation method of the present invention.

[0034] Among them, 1 is secondary brand BPA, 2 is crude BPA after drying, 3 is water, 4 is crude BPA after metering, 5 is crude BPA solution, 6 is crude BPA solution after primary filtration, 7 is BPA solution, 8 is BPA melt, 9 isopropyl ether circulation, 10 isolating tank, 11 is primary filter, 12 is secondary filter, 13 isolating tower, 14 is paddle dryer, 15 is metering tank. DETAILED DESCRIPTION

[0035] In order to better understand the technical solution of the present invention, the following examples will further illustrate the method provided by the present invention, but the present invention is not limited to the listed examples, and should also include any other known changes within the scope of the claims of the present invention.

[0036] like Figure 1 As shown, a method for pre-processing and productizing the recovery of secondary brand BPA comprises the following steps:

[0037] 1) The secondary brand BPA1 comes from the wastewater produced by the phosgenation process PC. The secondary brand BPA1 enters the paddle dryer 14 to remove water 3 to obtain the dried crude BPA2;

[0038] 2) The secondary brand BPA (i.e. the dried crude BPA 2) after the treatment in step 1) enters the metering tank 15; the metered crude BPA 4 enters the dissolving tank 10 with stirring, and the solvent is added to dissolve to obtain the BPA solution 5;

[0039] 3) The BPA solution 5 after the treatment in step 2) enters the primary filter 11 to remove solid particles larger than 20 μm;

[0040] 4) The BPA solution treated in step 3) (i.e., the crude BPA solution 6 after primary filtration) enters a secondary filter 12 to further remove solid particles;

[0041] 5) The BPA solution 7 after the treatment in step 4) enters the solvent recovery tower 13, where the solvent is removed and recovered, and the circulating isopropyl ether 9 is returned to the dissolving tank 10 to obtain a high-purity BPA melt 8 product.

[0042] In step 1), the secondary brand BPA, based on total mass, contains 8-20% water, 1-2% sodium chloride, 10-100 ppm ferric chloride, 1000-3000 ppm PC, and 78%-90% BPA.

[0043] The secondary brand BPA is preferably prepared by adjusting the pH of waste brine with a BPA content of 0.1-0.8 wt % to 1-6 in an acid precipitation tank to precipitate BPA particles, and filtering the waste brine through a rotary drum.

[0044] In step 1), a high-temperature gas is introduced as a carrier gas, and the temperature of the high-temperature gas is 100-140°C, preferably 110-120°C; BPA easily forms hydrogen bonds with water and is difficult to dry, and a high-temperature carrier gas is used to accelerate the drying speed. The high-temperature gas can be hot air or hot nitrogen, preferably hot nitrogen; the temperature of the high-temperature gas is 100-140°C, preferably 110-120°C; the drying temperature is 100-140°C, preferably 110-120°C, and the residence time is 0.1-5h, preferably 0.3-1h.

[0045] The amount of high temperature gas and secondary brand BPA is 0.1-1Nm 3 / kg, preferably 0.5-0.8Nm 3 / kg; the paddle dryer of the present invention may also be other forms of dryers, such as a tube dryer, a fluidized bed dryer, and a paddle dryer is preferably used.

[0046] In step 2), the solvent used can be methanol, ethanol, butanol, phenol, acetone, MTBE, isopropyl ether, preferably isopropyl ether; the mass concentration of BPA in the prepared solution is 10%-30%, preferably 20%-25%. The crude BPA after drying in step 1) enters the batching metering tank by gravity, and the batching tank is batched intermittently, and a certain amount of crude BPA is added to the metering tank each time, and then a certain amount of solvent is added to dissolve it.

[0047] In step 3), the primary filter used can be a filter bag or a filter rod, preferably a filter rod. The filter rod material can be, for example, 316L, polyphenylene sulfide, or PTFE, preferably polyphenylene sulfide. The filtration accuracy is 10-50 μm, preferably 20-30 μm. Solid particles larger than 10 microns can be removed through primary filtration, and the solid particle removal rate is above 95%.

[0048] In step 4), the secondary filter contains a nanofiltration membrane, and the purpose of the secondary filtration is to remove trace solid particles such as sodium chloride, ferric chloride, PC, etc.

[0049] The nanofiltration membrane has a three-layer structure, the bottom layer is a support layer made of PTFE material, the middle layer is a filter layer made of PVDF material, and the top layer is a protective layer made of PP material;

[0050] The filter layer has a thickness of 2-3 mm and a pore size of 20-30 nanometers;

[0051] The thickness of the protective layer is 1-2 mm, and the pore size is 10-20 microns.

[0052] In step 3), the distillation tower can be a plate tower, a structured packing tower, or a random packing tower, preferably a plate tower; the distillation process can refer to the distillation process of BPA in the prior art, for example, the distillation parameters are a theoretical plate number of 28, a reflux ratio of 0.5, a bottom pressure of 20 kPa, and a bottom temperature of 200 ° C.

[0053] In the present invention, the purity of the BPA product finally recovered is greater than 99.9%, the platinum-cobalt chromaticity is not greater than 5, the sodium chloride is not greater than 0.01ppm, the ferric chloride is less than 0.01ppm, and the PC is less than 0.01ppm. The BPA product of this purity can be used for the production of PC, and no longer needs to be treated as solid waste, thus realizing the productized recycling of secondary brand BPA.

[0054] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited thereto.

[0055] The source of the secondary brand BPA is: from waste brine with a BPA content of 0.1-0.8wt%, the pH is adjusted to 1-2 in an acid precipitation tank, BPA particles are precipitated, and filtered through a drum. The secondary brand BPA has a purity of 82%, a water content of 16%, sodium chloride of 1.5%, PC of 2000ppm, and ferric chloride of 58ppm.

[0056] BPA Testing Method:

[0057] BPA water content test: Take 1.5g of powder and accurately record the weighed mass. Put the powder into the special bottle of Karl Fischer furnace and press the bottle cap tightly. Connect the Karl Fischer furnace to the coulometric moisture meter. Set the Karl Fischer furnace heating treatment temperature to 120℃, and accurately enter the sample mass after measuring the blank to measure the water content.

[0058] BPA color number test: Take 15g of solid, accurately record the weight, add 150g of methanol, and dissolve evenly. Use a measuring cylinder to measure 50ml of liquid and add it to a colorimetric tube, and compare it with a platinum-cobalt colorimetric tube.

[0059] Sodium chloride test in BPA: Weigh 1g of solid, record the weight accurately, add it to a nickel dry pot, add 10g of aqua regia to digest at 250℃, dissolve for 30min, then add pure water to dilute to 100ml. Use ICP measurement.

[0060] PC measurement in BPA: Weigh 10g of solid, accurately record the weighed mass, add it to a disposable beaker, add 50g of methanol to dissolve for 30min, weigh it with 1-micron filter paper and filter it, dry it in an oven at 100℃ for 2h, accurately weigh the total mass of the filter paper and the filtrate; take 10mg of the filtrate and put it into a TG crucible for thermal weight loss at 250℃, the weight loss mass is the mass of PC.

[0061] Example 1

[0062] The secondary brand BPA from the previous process, containing 16% water, 1.5% sodium chloride, 82.3% BPA, 58ppm ferric chloride, and 2000ppm PC, enters the paddle dryer at a feed rate of 5kg / h. The dryer temperature is set at 110℃ and the pressure is 2.5Nm 3 / h nitrogen gas at 110°C was introduced to remove volatile water, and dried for 1 hour. The nitrogen gas entrained water and discharged into the air, and the dried crude BPA entered the metering tank. The water content of the crude BPA after drying was 30ppm.

[0063] The metering tank feeds the dried crude BPA into the dissolution tank at a rate of 4.2 kg / time, and adds isopropyl ether at a rate of 16.8 kg / time, and the crude BPA solution is obtained after mixing and dissolving. The crude BPA solution enters the primary filter at a rate of 21 kg / h, and the primary filter uses a filter rod made of 25 micron polyphenylene sulfide. After the primary filtration, the crude BPA solution enters the 25nm secondary filter. The secondary filter nanofiltration membrane has a 3-layer structure, the bottom layer is a 2mm thick PTFE membrane with a pore size of 50 microns, the middle layer is a 2mm thick PVDF material with a pore size of 25nm, and the top layer is a 2mm thick PP material with a pore size of 20 microns.

[0064] The BPA solution was fed into a distillation tower with a theoretical plate number of 35, a reflux ratio of 0.2, a bottom pressure of 20 kPa, and a bottom temperature of 200 ° C. Isopropyl ether was recovered from the top of the tower, and the BPA product was obtained from the bottom of the tower. The replacement cycle of the secondary filtration was 20 days, and the BPA color number was 3, sodium chloride 0.008 ppm, ferric chloride 0.008 ppm, PC 0.009 ppm, and isopropyl ether 10 ppm.

[0065] Example 2

[0066] The secondary brand BPA from the previous process, containing 9% water, 1% sodium chloride, 89.9% BPA, 100ppm ferric chloride, and 1000ppm PC, enters the paddle dryer at a feed rate of 5kg / h. The dryer temperature is set at 120℃ and the pressure is 4Nm 3 / h nitrogen gas at 120°C was introduced to remove volatile water, and dried for 0.3h. The nitrogen gas entrained water and discharged into the air, and the dried crude BPA entered the metering tank. The water content of the dried crude BPA was 20ppm.

[0067] The metering tank feeds the dried crude BPA into the dissolution tank at a rate of 4.55 kg / time, and MTBE is added at a rate of 13.65 kg / time, and the crude BPA solution is obtained after mixing and dissolving. The crude BPA solution enters the primary filter at a rate of 18.2 kg / h, and the primary filter uses a filter rod made of 20 micron polyphenylene sulfide. After the primary filtration, the crude BPA solution enters the 20nm secondary filter. The secondary filter nanofiltration membrane has a 3-layer structure, the bottom layer is a 3mm thick PTFE membrane with a pore size of 40 microns, the middle layer is a 3mm thick PVDF material with a pore size of 20nm, and the top layer is a 1mm thick PP material with a pore size of 10 microns.

[0068] The BPA solution was fed into a distillation tower with a theoretical plate number of 20, a reflux ratio of 2, a bottom pressure of 30 kPa, and a bottom temperature of 210°C. MTBE was recovered from the top of the tower, and BPA product was obtained from the bottom of the tower. The replacement cycle of the secondary filtration was 10 days, and the obtained BPA color number was 5, sodium chloride 0.005 ppm, ferric chloride 0.005 ppm, PC 0.006 ppm, and MTBE 15 ppm.

[0069] Example 3

[0070] The secondary brand BPA from the previous process, containing 20% ​​water, 2% sodium chloride, 77.7% BPA, 10ppm ferric chloride, and 3000ppm PC, enters the paddle dryer at a feed rate of 5kg / h. The dryer temperature is set at 115℃ and the pressure is 3.5Nm 3 / h nitrogen gas at 115°C was introduced to remove volatile water, and dried for 0.8h. The nitrogen gas entrained water and discharged into the air, and the dried crude BPA entered the metering tank. The water content of the crude BPA after drying was 25ppm.

[0071] The metering tank feeds the dried crude BPA into the dissolution tank at a rate of 4.0 kg / time, and butanol is added at a rate of 22.7 kg / time, and a crude BPA solution is obtained after mixing and dissolving. The crude BPA solution enters the primary filter at a rate of 26.7 kg / h, and the primary filter uses a filter rod made of 30 micron polyphenylene sulfide. After the primary filtration, the crude BPA solution enters the 30nm secondary filter. The secondary filter nanofiltration membrane has a 3-layer structure, the bottom layer is a 3mm thick PTFE membrane with a pore size of 40 microns, the middle layer is a 3mm thick PVDF material with a pore size of 30nm, and the top layer is a 2mm thick PP material with a pore size of 20 microns.

[0072] The BPA solution was fed into a distillation tower with a theoretical plate number of 30, a reflux ratio of 1, a bottom pressure of 10 kPa, and a bottom temperature of 190°C. Butanol was recovered from the top of the tower, and the BPA product was obtained from the bottom of the tower. The secondary filtration replacement cycle was 10 days, and the BPA color number was 5, sodium chloride 0.01 ppm, ferric chloride 0.009 ppm, PC 0.009 ppm, and butanol 12 ppm were obtained.

[0073] Comparative Example 1

[0074] The secondary brand BPA from the previous process contains 20% water, 2% sodium chloride, 77.7% BPA, 10ppm ferric chloride, and 3000ppm PC. It enters the paddle dryer at a feed rate of 5kg / h. The dryer temperature is set at 150℃ and dried for 1.5h. The dried crude BPA enters the metering tank. The water content of the dried crude BPA is 65ppm.

[0075] The metering tank feeds the dried crude BPA into the dissolution tank at a rate of 4.0 kg / time, and adds isopropyl ether at a rate of 12 kg / time, and the crude BPA solution is obtained after mixing and dissolving. The crude BPA solution enters the primary filter at a rate of 16 kg / h, and the primary filter uses a filter rod made of 100 micron polyphenylene sulfide. After the primary filtration, the crude BPA solution enters the 30nm secondary filter. The secondary filter nanofiltration membrane has a 3-layer structure, the bottom layer is a 3mm thick PTFE membrane with a pore size of 40 microns, the middle layer is a 3mm thick PVDF material with a pore size of 30nm, and the top layer is a 2mm thick PP material with a pore size of 20 microns.

[0076] The BPA solution was fed into a distillation tower with a theoretical plate number of 15, a reflux ratio of 3, a bottom pressure of 5 kPa, and a bottom temperature of 180°C. Isopropyl ether was recovered from the top of the tower, and the BPA product was obtained from the bottom of the tower. The replacement cycle of the secondary filtration was 0.1 days, and the BPA color number was 3, sodium chloride 0.012 ppm, ferric chloride 0.009 ppm, PC 0.009 ppm, and isopropyl ether 50 ppm.

[0077] Comparative Example 2

[0078] The secondary brand BPA from the previous process, containing 20% ​​water, 2% sodium chloride, 77.7% BPA, 10ppm ferric chloride, and 3000ppm PC, enters the paddle dryer at a feed rate of 5kg / h. The dryer temperature is set at 90℃ and the pressure is 5Nm 3 / h nitrogen gas at 90°C was introduced to remove volatile water, and dried for 1 hour. The nitrogen gas entrained water and discharged into the air, and the dried crude BPA entered the metering tank. The water content of the crude BPA after drying was 105ppm.

[0079] The metering tank feeds the dried crude BPA into the dissolution tank at a rate of 4.0 kg / time, and adds isopropyl ether at a rate of 12 kg / time, and the crude BPA solution is obtained after mixing and dissolving. The crude BPA solution enters the primary filter at a rate of 16 kg / h, and the primary filter uses a filter rod made of 30 micron polyphenylene sulfide. After the primary filtration, the crude BPA solution enters the 30nm secondary filter. The secondary filter nanofiltration membrane has a 3-layer structure, the bottom layer is a 3mm thick PTFE membrane with a pore size of 40 microns, the middle layer is a 3mm thick PP material with a pore size of 30nm, and the top layer is a 2mm thick PP material with a pore size of 20 microns.

[0080] The BPA solution was fed into a distillation tower with a theoretical plate number of 20, a reflux ratio of 1, a bottom pressure of 20 kPa, and a bottom temperature of 200 ° C. Isopropyl ether was recovered from the top of the tower, and the BPA product was obtained from the bottom of the tower. The secondary filtration replacement cycle was 1 day, and the BPA color number was 10, sodium chloride 0.05 ppm, ferric chloride 0.009 ppm, PC 0.009 ppm, and isopropyl ether 16 ppm.

[0081] Comparative Example 3

[0082] The secondary brand BPA from the previous process, containing 20% ​​water, 2% sodium chloride, 77.7% BPA, 10ppm ferric chloride, and 3000ppm PC, enters the paddle dryer at a feed rate of 5kg / h. The dryer temperature is set at 120℃ and the pressure is 3.5Nm 3 / h nitrogen gas at 120°C is introduced to remove volatile water and dried for 1 hour. The nitrogen gas carries water and is discharged into the air. The dried crude BPA enters the metering tank.

[0083] The metering tank feeds the dried crude BPA into the dissolution tank at a rate of 4.0 kg / time, and adds isopropyl ether at a rate of 12 kg / time, and the crude BPA solution is obtained after mixing and dissolving. The crude BPA solution enters the primary filter at a rate of 16 kg / h, and the primary filter uses a filter rod made of 30 micron polyphenylene sulfide. After the primary filtration, the crude BPA solution enters the 50nm secondary filter. The secondary filter nanofiltration membrane has a 3-layer structure, the bottom layer is a 3mm thick PTFE membrane with a pore size of 40 microns, the middle layer is a 3mm thick PVDF material with a pore size of 50nm, and the top layer is a 2mm thick PP material with a pore size of 20 microns.

[0084] The BPA solution was fed into a distillation tower with a theoretical plate number of 20, a reflux ratio of 1, a bottom pressure of 20 kPa, and a bottom temperature of 200 ° C. Isopropyl ether was recovered from the top of the tower, and the BPA product was obtained from the bottom of the tower. The secondary filtration replacement cycle was 10 days, and the BPA color number was 15, sodium chloride 0.012 ppm, ferric chloride 0.03 ppm, PC 0.03 ppm, and isopropyl ether 16 ppm.

[0085] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as limiting the present invention. Those skilled in the art will appreciate that, under the guidance of this specification, some modifications or adjustments may be made to the present invention. These modifications or adjustments should also be within the scope defined by the claims of the present invention.

Claims

1. A method for recycling secondary brand BPA by pretreatment and productization, characterized in that: The following steps are involved: 1) Wastewater containing secondary brand BPA produced by phosgenation PC enters a dryer to remove moisture; In step 1), a high-temperature gas is introduced as a carrier gas, and the temperature of the high-temperature gas is 100-140°C; 2) The secondary brand BPA treated in step 1) is placed in a dissolving tank with stirring, and a solvent is added to dissolve it to obtain a BPA solution; 3) The BPA solution obtained in step 2) enters a primary filter to remove solid particles larger than 20 μm; 4) The BPA solution after the treatment in step 3) enters the secondary filter to further remove solid particles; the secondary filter in step 4) includes a nanofiltration membrane; the nanofiltration membrane has a three-layer structure, the bottom layer is a support layer made of PTFE material, the middle layer is a filter layer made of PVDF material, and the top layer is a protective layer made of PP material; the support layer is 2-3mm thick and has a pore size of 40-50 microns; the filter layer is 2-3mm thick and has a pore size of 20-30 nanometers; the protective layer is 1-2mm thick and has a pore size of 10-20 microns; 5) The BPA solution after the treatment in step 4) enters a distillation tower to remove and recover the solvent to obtain a high-purity BPA product.

2. The method according to claim 1, characterized in that The secondary brand BPA in step 1) contains, by total mass, 8-20% water, 1-2% sodium chloride, 10-100 ppm ferric chloride, 1000-3000 ppm PC, and 78%-90% BPA.

3. The method according to claim 1 or 2, characterized in that: The temperature of the high temperature gas in step 1) is 110-120°C.

4. The method according to claim 3, characterized in that The amount of high temperature gas and secondary brand BPA is 0.1-1Nm 3 / kg.

5. The method according to claim 4, characterized in that The amount of high temperature gas and secondary brand BPA is 0.5-0.8Nm 3 / kg.

6. The method according to claim 3, characterized in that: The high temperature gas is selected from hot air or hot nitrogen.

7. The method according to claim 6, characterized in that The high temperature gas is hot nitrogen.

8. The method according to claim 3, characterized in that The dryer is selected from any one of a paddle dryer, a tube dryer, and a fluidized bed dryer.

9. The method according to claim 8, characterized in that The dryer is a paddle dryer.

10. The method according to claim 3, characterized in that In step 1), the drying temperature is 100-140° C. and the residence time is 0.1-5 h.

11. The method according to claim 10, characterized in that In step 1), the drying temperature is 110-120° C. and the residence time is 0.3-1 h.

12. The method according to claim 1 or 2, characterized in that: The solvent in step 2) is selected from at least one of methanol, ethanol, butanol, phenol, acetone, MTBE, and isopropyl ether.

13. The method according to claim 12, characterized in that The solvent in step 2) is isopropyl ether.

14. The method according to claim 12, characterized in that The mass concentration of BPA in the prepared solution is 10%-30%.

15. The method according to claim 14, characterized in that The mass concentration of BPA in the prepared solution is 20%-25%.

16. The method according to claim 1 or 2, characterized in that: The primary filter in step 3) is a filter bag or a filter rod.

17. The method according to claim 16, characterized in that The primary filter in step 3) is a filter stick.

18. The method according to claim 16, characterized in that The filter rod material is selected from any one of 316L, polyphenylene sulfide, and PTFE.

19. The method according to claim 18, characterized in that The filter rod is made of polyphenylene sulfide.

20. The method according to claim 16, characterized in that The filtration accuracy in step 3) is 10-50 μm.

21. The method according to claim 20, characterized in that The filtration accuracy in step 3) is 20-30 μm.

22. The method according to claim 1 or 2, characterized in that In step 5), the distillation tower is selected from any one of a plate tower, a structured packing tower, and a random packing tower.

23. The method according to claim 22, characterized in that In step 5), the distillation tower is a plate tower.

24. The method according to claim 22, characterized in that The number of theoretical plates of the distillation tower is 20-35, the reflux ratio is 0.2-2, the bottom pressure is 10-30 kPa, and the bottom temperature is 190-210°C.

25. The method according to claim 1 or 2, characterized in that Step 5) The purity of the high-purity BPA product obtained is greater than 99.9%, the platinum-cobalt chromaticity is not greater than 5, the sodium chloride is not greater than 0.01 ppm, the ferric chloride is less than 0.01 ppm, and the PC is less than 0.01 ppm.

Citation Information

Patent Citations

  • Little nanofiltration membrane

    CN205914032U

  • Bisphenol A preparation method