A long-acting antibacterial agent and its preparation method
By using composite modification treatments such as chitosan, nano-titanium dioxide, and copper ions, the bonding strength between the antibacterial agent and the fabric is enhanced, solving the problem of easy detachment of the antibacterial agent and achieving long-lasting antibacterial effect and regeneration capability.
Patent Information
- Application Number
- CN202311488944.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-09
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-11-09
AI Technical Summary
Existing antibacterial agents have low bonding strength to textiles, are easy to fall off, and have a short antibacterial duration, making it difficult to maintain long-term antibacterial properties during friction and washing.
A composite method using chitosan, nano-titanium dioxide, copper ions, and halogenated amine groups was adopted. The binding strength of the antibacterial agent was improved through modification treatment, and a network structure was formed through polymerization reaction, which enhanced the bonding strength between the antibacterial agent and the fabric.
It achieves high bonding strength between the antibacterial agent and the fabric, prolongs the antibacterial effect, and maintains good antibacterial performance even after multiple washes and UV irradiation, and also has regeneration capabilities.
Smart Images

Figure BDA0004540612990000161 
Figure BDA0004540612990000171 
Figure BDA0004540612990000172
Abstract
Description
Technical Field
[0001] This invention relates to the field of antibacterial technology, and more specifically, to a long-acting antibacterial agent and its preparation method. Background Technology
[0002] Antimicrobial agents are substances or products with bacteriostatic and bactericidal properties. They come in many varieties, such as silver ion antimicrobial agents, nano-antimicrobial agents, heavy metal ions, chitosan, peptides, quaternary ammonium salts, and halogenated amines. Antimicrobial agents have wide applications in the food, medical, and textile industries.
[0003] In the textile industry, antibacterial agents can be added to the finishing and dyeing solutions during fabric preparation. This allows the antibacterial agents to adhere to the fabric fibers, either directly or by coating them onto the fibers, thus giving the fabric a certain degree of antibacterial and sterilizing properties. Due to the special nature of fabrics, they are subject to pleating, friction, and repeated washing during use. During these processes, the antibacterial agents on the fabric will detach, directly affecting the fabric's long-term antibacterial properties.
[0004] Patent 202010880442.5 discloses a method for preparing a betaine-haloamine compound dual antibacterial textile. The method involves adding a betaine antibacterial agent containing carbon-carbon double bonds and a haloamine precursor compound containing carbon-carbon double bonds to an organic solvent to prepare a finishing solution. Textiles are then added to this solution for impregnation. The impregnated textiles are placed in an electron beam irradiation device for electron radiation grafting reaction. After washing and drying, the textiles are immersed in a sodium hypochlorite aqueous solution for chlorination. After washing and drying, an antibacterial textile is obtained. This textile possesses dual antibacterial properties of haloamine and betaine, resulting in improved antibacterial efficiency. However, in this technical solution, the haloamine antibacterial agent is easily decomposed under ultraviolet light, thus losing its antibacterial properties and resulting in a short antibacterial time. Furthermore, the binding strength between the haloamine and betaine antibacterial agents and the fabric is low, which is not conducive to the long-term loading of the antibacterial agent onto the fabric.
[0005] Patent 202211733862.6 discloses an antibacterial agent for textiles containing graphene and quaternary ammonium salts, and its preparation method. The method utilizes a dual-coupling agent to modify graphene, which is then reacted with dimethyl diallyl ammonium chloride, carboxylic acid monomers, and allyl glycidyl ether to obtain an antibacterial agent composed of a quaternary ammonium salt copolymer and graphene. This agent possesses the antibacterial properties of both organic and inorganic materials, imparting excellent antibacterial performance to the fabric. Furthermore, the antibacterial finishing agent contains active groups that can interact with cotton fibers, increasing the bonding strength between the antibacterial agent and the fabric, thereby achieving a long-lasting antibacterial effect. However, in this technical solution, the quaternary ammonium salt and graphene antibacterial agent lack renewability. With increasing usage time, the antibacterial agent is difficult to regenerate, thus limiting the antibacterial duration of the fabric. Summary of the Invention
[0006] The purpose of this invention is to provide a long-acting antibacterial agent. This antibacterial agent can enhance the antibacterial effect and effectively prolong the antibacterial duration through the synergistic effect of multiple antibacterial groups. Moreover, the antibacterial groups have a high bonding strength with the chitosan matrix and are not easy to fall off.
[0007] Another objective of this invention is to provide a method for preparing a long-acting antibacterial agent, which has simple procedures and mild reaction conditions.
[0008] The technical problem solved by this invention is achieved by the following technical solution.
[0009] On one hand, embodiments of the present invention provide a method for preparing a long-acting antibacterial agent, comprising the following steps:
[0010] S1: Mix chitosan with an aqueous acetic acid solution and stir at 50-60℃ to dissolve the chitosan; then add 2,3-epoxypropyltrimethylammonium chloride. After the reaction is complete, add a copper ion salt solution to the system, stir evenly, and adjust the pH value to 5-6 to obtain mixture A.
[0011] S2: Disperse nano-titanium dioxide in an aqueous ethanol solution, add γ-methacryloyloxypropyltrimethoxysilane, heat and stir; then add a haloamine precursor compound to the system to obtain mixture B;
[0012] S3: Mix the mixture A prepared in step S1 with the mixture B prepared in step S2, stir evenly, add an initiator, and disperse by ultrasonication; then add sodium hypochlorite solution, disperse by ultrasonication at 30-40℃ and stir for 8-10 hours to obtain the long-acting antibacterial agent.
[0013] Furthermore, in step S2, the preparation method of the nano-titanium dioxide includes the following steps: dissolving tetraisopropyl titanate and titanate coupling agent in dichloromethane, stirring evenly, then adding an aqueous solution of sodium dodecyl sulfonate and hexadecyltrimethylammonium chloride, stirring at high speed, then adding an aqueous solution of tetramethylguanidine, adjusting the pH value to 7-8, drying, and calcining.
[0014] Hollow spherical nano-titanium dioxide was prepared by this method. The hollow nano-titanium dioxide has a large specific surface area, which is beneficial for the loading of γ-methacryloxypropyltrimethoxysilane. The groups in γ-methacryloxypropyltrimethoxysilane can enter the micropores, thereby improving the physical connection between the two.
[0015] Furthermore, in step S3, a polyvinyl alcohol solution is first added and stirred until homogeneous, followed by the addition of a sodium hypochlorite solution. By adding polyvinyl alcohol, the molecular weights of polyvinyl alcohol and chitosan intertwine, and the hydroxyl groups form hydrogen bonds with the chitosan molecules, making the polyvinyl alcohol less prone to detachment. Moreover, polyvinyl alcohol increases the number of hydroxyl groups on chitosan, making the antibacterial agent more hydrophilic. Furthermore, during use, the hydroxyl groups of the antibacterial agent form hydrogen bonds with hydroxyl and carboxyl groups in the fabric fibers, increasing the bonding strength between the antibacterial agent and the fabric, thus preventing the antibacterial agent from detaching from the fabric. This extends the antibacterial effect of the antibacterial fabric.
[0016] Furthermore, in step S1, after adding copper ion salt solution and stirring evenly, aluminum chloride aqueous solution is added, ultrasonically dispersed at 50-60°C, and then allowed to stand.
[0017] Adding an aqueous solution of aluminum chloride to the chitosan system has a flocculating effect. During this step, aluminum hydroxide or polyaluminum chloride can carry some copper ions and deposit them on the chitosan, thus grafting aluminum ions onto the chitosan. During the use of the antibacterial agent, aluminum ions can enter the interior of the fabric fibers, thereby improving the bonding strength between the antibacterial agent and the fabric.
[0018] Furthermore, the mass ratio of copper ions in the copper ion salt solution to the mass ratio of aluminum ions in the aluminum chloride aqueous solution is 1:(0.5-1).
[0019] Furthermore, the haloamine precursor compound is one or more of 3-allyl-5,5-dimethylhydantoin, 1-allylhydantoin, and 3-(4'-vinylbenzyl)-5,5-dimethylhydantoin.
[0020] Furthermore, the initiator is one or more of sodium persulfate, potassium persulfate, and ammonium persulfate;
[0021] The copper ion salt is one or more of copper nitrate, copper sulfate, and copper chloride.
[0022] Furthermore, in step S1, the mass ratio of chitosan to 2,3-epoxypropyltrimethylammonium chloride is 1:5-8. By adding an excess of 2,3-epoxypropyltrimethylammonium chloride, the chitosan is fully quaternized to obtain sufficient quaternary ammonium salt groups.
[0023] Furthermore, in step S2, the mass ratio of nano-titanium dioxide to γ-methacryloxypropyltrimethoxysilane is 1:30-40, and the mass ratio of nano-titanium dioxide to the haloamine precursor compound is 1:4-5. An excess of coupling agent is added to ensure that all titanium dioxide is modified, thereby improving its utilization rate. Similarly, adding an excess of the haloamine precursor compound allows for full utilization of titanium dioxide, and the excess haloamine precursor compound also plays an antibacterial role.
[0024] On the other hand, embodiments of the present invention provide a long-acting antibacterial agent, which is prepared by the above-described method.
[0025] Compared with the prior art, the embodiments of the present invention have at least the following advantages or beneficial effects:
[0026] In this application, chitosan is first modified with 2,3-epoxypropyltrimethylammonium chloride to obtain quaternized chitosan. Then, the quaternized chitosan is mixed with a copper ion salt solution, and the copper ions complex with the quaternized chitosan, so that the copper ions are negatively attached to the chitosan molecular chain. At the same time, since the chitosan molecular chain has a certain encapsulation effect, the copper ions are encapsulated, thereby improving the binding strength between the copper ions and chitosan.
[0027] In step S2, γ-methacryloxypropyltrimethoxysilane is used to modify nano-titanium dioxide, thereby improving the reactivity of nano-titanium dioxide. Under the action of the initiator added in step S3, the haloamine precursor compound undergoes a polymerization reaction with γ-methacryloxypropyltrimethoxysilane, chitosan, and other raw materials to form long-chain haloamine substances. At the same time, chitosan molecules themselves cross-link and entangle to form a network structure, and the long-chain haloamine substances also cross-link and entangle on the network structure, thereby improving the binding strength between haloamine groups and chitosan. Furthermore, quaternary ammonium salt groups and copper ion groups are grafted onto chitosan molecules. During the action of the initiator, as chitosan molecules cross-link and entangle, their binding strength with the chitosan network structure is also enhanced.
[0028] In summary, this application combines nano-titanium dioxide, copper ions, quaternary ammonium salts, and haloamine groups onto a network of chitosan, significantly improving the bonding strength between these groups. This prevents the groups from easily detaching during use, thus achieving a long-lasting antibacterial effect. Furthermore, the antibacterial agent of this application combines chitosan, heavy metal ions, quaternary ammonium salts, and haloamine groups. The synergistic effect of multiple antibacterial substances means that when halide ions or heavy metal ions in the haloamine groups are lost, the remaining antibacterial substances can act as substitutes, thereby extending the antibacterial duration of the agent. Detailed Implementation
[0029] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.
[0030] It should be noted that, unless otherwise specified, the embodiments and features described in the present invention can be combined with each other. The present invention will now be described in detail with reference to specific embodiments.
[0031] The features and performance of the present invention will be further described in detail below with reference to embodiments.
[0032] Example 1
[0033] Prepare the antibacterial agent according to the following steps:
[0034] S1: Chitosan with a molecular weight of 50,000-60,000 Da is mixed with a 0.03 mg / ml dilute acetic acid aqueous solution. The mixture is heated in a water bath, and the temperature of the solution is controlled at 50±1℃. The mixture is stirred to dissolve the chitosan, resulting in a 0.02 mg / ml chitosan acetic acid solution. Then, 2,3-epoxypropyltrimethylammonium chloride is added to the solution, and the mixture is stirred. After the reaction is complete, a 10% copper nitrate solution is added to the system, and the mixture is stirred until homogeneous. The pH value is adjusted to 6 to obtain mixture A. The mass ratio of chitosan to 2,3-epoxypropyltrimethylammonium chloride is 1:8, and the mass ratio of copper ions to chitosan is 2:1.
[0035] S2: Dissolve 100g tetraisopropyl titanate and 5g titanate coupling agent in sufficient dichloromethane, stir evenly, then add 20g sodium dodecyl sulfonate and 10g hexadecyltrimethylammonium chloride aqueous solution while stirring at high speed, then add 15% tetramethylguanidine aqueous solution, adjust the pH value to 7, dry, and calcine at 650℃ to obtain nano titanium dioxide;
[0036] The above-mentioned nano-titanium dioxide was dispersed in a sufficient amount of 50% (v / v) aqueous ethanol solution, and γ-methacryloxypropyltrimethoxysilane was added. The mixture was heated to 50±1℃ and stirred. Then, 3-allyl-5,5-dimethylhydantoin was added to the system and stirred until homogeneous to obtain mixture B. The mass ratio of nano-titanium dioxide to γ-methacryloxypropyltrimethoxysilane was 1:30, and the mass ratio of nano-titanium dioxide to 3-allyl-5,5-dimethylhydantoin was 1:4.
[0037] S3: Mix the mixture A prepared in step S1 with the mixture B prepared in step S2, stir evenly, add sodium persulfate powder, and ultrasonically disperse for 2 hours; then add a sodium hypochlorite solution with a mass fraction of 0.2%, ultrasonically disperse and stir for 8 hours at 30±1℃; to obtain the long-acting antibacterial agent.
[0038] The mass of sodium persulfate powder is 2% of the total mass of 3-allyl-5,5-dimethylhydantoin and γ-methacryloyloxypropyltrimethoxysilane. The volume ratio of sodium hypochlorite solution to the volume of mixture A and B is 1:1.
[0039] Example 2
[0040] Prepare the antibacterial agent according to the following steps:
[0041] S1: Chitosan with a molecular weight of 50,000-60,000 Da is mixed with a 0.03 mg / ml dilute acetic acid aqueous solution. The mixture is heated in a water bath, and the temperature of the solution system is controlled at 55±1℃. The mixture is stirred to dissolve the chitosan, resulting in a 0.02 mg / ml chitosan acetic acid solution. Then, 2,3-epoxypropyltrimethylammonium chloride is added to the solution system and stirred. After the reaction is complete, a 10% copper nitrate solution is added to the system and stirred until homogeneous. The pH value is adjusted to 5 to obtain mixture A. The mass ratio of chitosan to 2,3-epoxypropyltrimethylammonium chloride is 1:6, and the mass ratio of copper ions to chitosan is 2:1.
[0042] S2: Dissolve 100g tetraisopropyl titanate and 5g titanate coupling agent in sufficient dichloromethane, stir evenly, then add 20g sodium dodecyl sulfonate and 10g hexadecyltrimethylammonium chloride aqueous solution while stirring at high speed, then add 15% tetramethylguanidine aqueous solution, adjust the pH value to 7, dry, and calcine at 650℃ to obtain nano titanium dioxide;
[0043] The above-mentioned nano-titanium dioxide was dispersed in a sufficient amount of 50% (v / v) aqueous ethanol solution, and γ-methacryloxypropyltrimethoxysilane was added. The mixture was heated to 50±1℃ and stirred. Then, 3-allyl-5,5-dimethylhydantoin was added to the system and stirred until homogeneous to obtain mixture B. The mass ratio of nano-titanium dioxide to γ-methacryloxypropyltrimethoxysilane was 1:35, and the mass ratio of nano-titanium dioxide to 3-allyl-5,5-dimethylhydantoin was 1:5.
[0044] S3: Mix the mixture A prepared in step S1 with the mixture B prepared in step S2, stir evenly, add potassium persulfate powder, and ultrasonically disperse for 2 hours; then add sodium hypochlorite solution with a mass fraction of 0.2%, ultrasonically disperse and stir for 8 hours at 35±1℃; to obtain the long-acting antibacterial agent.
[0045] The mass of sodium persulfate powder is 2% of the total mass of 3-allyl-5,5-dimethylhydantoin and γ-methacryloyloxypropyltrimethoxysilane added. The volume ratio of sodium hypochlorite solution to mixture A and B is 0.9:1.
[0046] Example 3
[0047] Prepare the antibacterial agent according to the following steps:
[0048] S1: Chitosan with a molecular weight of 50,000-60,000 Da is mixed with a 0.03 mg / ml dilute acetic acid aqueous solution. The mixture is heated in a water bath, and the temperature of the solution is controlled at 50±1℃. The mixture is stirred to dissolve the chitosan, resulting in a 0.02 mg / ml chitosan acetic acid solution. Then, 2,3-epoxypropyltrimethylammonium chloride is added to the solution, and the mixture is stirred. After the reaction is complete, a 10% copper nitrate solution is added to the system, and the mixture is stirred until homogeneous. The pH value is adjusted to 5 to obtain mixture A. The mass ratio of chitosan to 2,3-epoxypropyltrimethylammonium chloride is 1:7, and the mass ratio of copper ions to chitosan is 2:1.
[0049] S2: Dissolve 100g tetraisopropyl titanate and 5g titanate coupling agent in sufficient dichloromethane, stir evenly, then add 20g sodium dodecyl sulfonate and 10g hexadecyltrimethylammonium chloride aqueous solution while stirring at high speed, then add 15% tetramethylguanidine aqueous solution, adjust the pH value to 7, dry, and calcine at 650℃ to obtain nano titanium dioxide;
[0050] The above-mentioned nano-titanium dioxide was dispersed in a sufficient amount of 50% (v / v) aqueous ethanol solution, and γ-methacryloxypropyltrimethoxysilane was added. The mixture was heated to 50±1℃ and stirred. Then, 3-allyl-5,5-dimethylhydantoin was added to the system and stirred until homogeneous to obtain mixture B. The mass ratio of nano-titanium dioxide to γ-methacryloxypropyltrimethoxysilane was 1:40, and the mass ratio of nano-titanium dioxide to 3-allyl-5,5-dimethylhydantoin was 1:4.5.
[0051] S3: Mix the mixture A prepared in step S1 with the mixture B prepared in step S2, stir evenly, add sodium persulfate powder, and ultrasonically disperse for 2 hours; then add a sodium hypochlorite solution with a mass fraction of 0.3%, ultrasonically disperse and stir for 9 hours at 30±1℃; to obtain the long-acting antibacterial agent.
[0052] The mass of sodium persulfate powder is 2% of the total mass of 3-allyl-5,5-dimethylhydantoin and γ-methacryloyloxypropyltrimethoxysilane added. The volume ratio of sodium hypochlorite solution to mixture A and B is 0.8:1.
[0053] Example 4
[0054] Prepare the antibacterial agent according to the following steps:
[0055] S1: Chitosan with a molecular weight of 50,000-60,000 Da is mixed with a 0.03 mg / ml dilute acetic acid aqueous solution. The mixture is heated in a water bath, and the temperature of the solution is controlled at 50±1℃. The mixture is stirred to dissolve the chitosan, resulting in a 0.02 mg / ml chitosan acetic acid solution. Then, 2,3-epoxypropyltrimethylammonium chloride is added to the solution, and the mixture is stirred. After the reaction is complete, a 10% copper nitrate solution is added to the system, and the mixture is stirred until homogeneous. The pH value is adjusted to 5 to obtain mixture A. The mass ratio of chitosan to 2,3-epoxypropyltrimethylammonium chloride is 1:5, and the mass ratio of copper ions to chitosan is 2:1.
[0056] S2: Dissolve 100g tetraisopropyl titanate and 5g titanate coupling agent in sufficient dichloromethane, stir evenly, then add 20g sodium dodecyl sulfonate and 10g hexadecyltrimethylammonium chloride aqueous solution while stirring at high speed, then add 15% tetramethylguanidine aqueous solution, adjust the pH value to 7, dry, and calcine at 650℃ to obtain nano titanium dioxide;
[0057] The above-mentioned nano-titanium dioxide was dispersed in a sufficient amount of 50% (v / v) aqueous ethanol solution, and γ-methacryloxypropyltrimethoxysilane was added. The mixture was heated to 50±1℃ and stirred. Then, 3-allyl-5,5-dimethylhydantoin was added to the system and stirred until homogeneous to obtain mixture B. The mass ratio of nano-titanium dioxide to γ-methacryloxypropyltrimethoxysilane was 1:40, and the mass ratio of nano-titanium dioxide to 3-allyl-5,5-dimethylhydantoin was 1:5.
[0058] S3: Mix the mixture A prepared in step S1 with the mixture B prepared in step S2, stir evenly, add sodium persulfate powder, and ultrasonically disperse for 2 hours; then add a sodium hypochlorite solution with a mass fraction of 0.5%, ultrasonically disperse and stir for 10 hours at 30±1℃; to obtain the long-acting antibacterial agent.
[0059] The mass of sodium persulfate powder is 2% of the total mass of 3-allyl-5,5-dimethylhydantoin and γ-methacryloyloxypropyltrimethoxysilane. The volume ratio of sodium hypochlorite solution to mixture A and B is 1:1.
[0060] Example 5
[0061] The difference from Example 1 is that step S3 is:
[0062] S3: Mix mixture A prepared in step S1 with mixture B prepared in step S2, stir evenly, add sodium persulfate powder, and ultrasonically disperse for 2 hours; first add a 10% (w / w) low-polymerization degree polyvinyl alcohol aqueous solution, stir evenly, then add sufficient sodium hypochlorite solution with a 0.1% (w / w) mass fraction, ultrasonically disperse and stir for 8 hours at 30±1℃; wherein the mass of sodium persulfate powder is 2% of the total mass of 3-allyl-5,5-dimethylhydantoin and γ-methacryloyloxypropyltrimethoxysilane added. The volume ratio of polyvinyl alcohol aqueous solution to mixture A and B is 1:1, and the volume ratio of sodium hypochlorite solution to mixture A and B is 0.8:1.
[0063] The remaining steps are the same as in Example 1.
[0064] Example 6
[0065] The difference from Example 1 is that step S1 is:
[0066] S1: Chitosan with a molecular weight of 50,000-60,000 Da was mixed with a 0.03 mg / ml dilute acetic acid aqueous solution. The mixture was heated in a water bath, and the temperature of the solution was controlled at 50±1℃. The mixture was stirred to dissolve the chitosan, resulting in a 0.02 mg / ml chitosan acetic acid solution. Then, 2,3-epoxypropyltrimethylammonium chloride was added to the solution, and the mixture was stirred until the reaction was complete. Next, a 10% (w / w) copper nitrate solution was added to the system, and the mixture was stirred until homogeneous. Then, a 1% (w / w) aluminum chloride aqueous solution was added, and the mixture was ultrasonically dispersed at 60℃. After standing, the pH was adjusted to 6 to obtain mixture A. The mass ratio of chitosan to 2,3-epoxypropyltrimethylammonium chloride was 1:8, and the mass ratio of copper ions to chitosan was 2:1. The volume ratio of the aluminum chloride aqueous solution to the chitosan acetic acid solution was 0.6:1.
[0067] The remaining steps are the same as in Example 1.
[0068] Example 7
[0069] The difference from Example 1 is that steps S1 and S3 are respectively:
[0070] S1: Chitosan with a molecular weight of 50,000-60,000 Da was mixed with a 0.03 mg / ml dilute acetic acid aqueous solution. The mixture was heated in a water bath, and the temperature of the solution was controlled at 50±1℃. The mixture was stirred to dissolve the chitosan, resulting in a 0.02 mg / ml chitosan acetic acid solution. Then, 2,3-epoxypropyltrimethylammonium chloride was added to the solution, and the mixture was stirred until the reaction was complete. Next, a 10% (w / w) copper nitrate solution was added to the system, and the mixture was stirred until homogeneous. Then, a 1% (w / w) aluminum chloride aqueous solution was added, and the mixture was ultrasonically dispersed at 60℃. After standing, the pH was adjusted to 6 to obtain mixture A. The mass ratio of chitosan to 2,3-epoxypropyltrimethylammonium chloride was 1:8, and the mass ratio of copper ions to chitosan was 2:1. The volume ratio of the aluminum chloride aqueous solution to the chitosan acetic acid solution was 0.6:1.
[0071] S3: Mix mixture A prepared in step S1 with mixture B prepared in step S2, stir evenly, add sodium persulfate powder, and ultrasonically disperse for 2 hours; first add a 10% (w / w) low-polymerization degree polyvinyl alcohol aqueous solution, stir evenly, then add sufficient sodium hypochlorite solution with a 0.1% (w / w) mass fraction, ultrasonically disperse and stir for 8 hours at 30±1℃; wherein the mass of sodium persulfate powder is 2% of the total mass of 3-allyl-5,5-dimethylhydantoin and γ-methacryloyloxypropyltrimethoxysilane added. The volume ratio of polyvinyl alcohol aqueous solution to mixture A and B is 1:1, and the volume ratio of sodium hypochlorite solution to mixture A and B is 0.8:1.
[0072] The remaining steps are the same as in Example 1.
[0073] Example 8
[0074] The difference from Example 7 is that in this example, the mass ratio of copper ions to aluminum ions in the aluminum chloride aqueous solution is 1:0.5, and the rest is the same as in Example 7.
[0075] Example 9
[0076] The difference from Example 7 is that in this example, the ratio of copper ions to aluminum ions in the aluminum chloride aqueous solution is 1:1. Everything else is the same as in Example 7.
[0077] Example 10
[0078] The difference from Example 7 is that the copper sulfate solution used in this example is the same as in Example 7.
[0079] Example 11
[0080] The difference from Example 1 is that in this example, the haloamine precursor compound is 1-allylhydantoin, the initiator is potassium persulfate, and the remaining steps are the same as in Example 1.
[0081] Example 12
[0082] The difference from Example 1 is that in this example, the halogenated amine precursor compound is 3-(4'-vinylbenzyl)-5,5-dimethylhydantoin, the initiator is ammonium persulfate, and the remaining steps are the same as in Example 1.
[0083] Example 13
[0084] The difference from Example 1 is that in this example, the haloamine precursor compound is a mixture of 3-(4'-vinylbenzyl)-5,5-dimethylhydantoin and 3-allyl-5,5-dimethylhydantoin in a mass ratio of 1:1, and the remaining steps are the same as in Example 1.
[0085] Example 14
[0086] The difference from Example 1 is that in this example, the haloamine precursor compound is a mixture of 1-allylhydantoin and 3-allyl-5,5-dimethylhydantoin in a mass ratio of 1:1, and the remaining steps are the same as in Example 1.
[0087] Example 15
[0088] The difference from Example 1 is that in this example, the nano titanium dioxide used in step S2 is purchased directly from the market. It is purchased from Tianjin Gaoke New Material Technology Co., Ltd., which produces red goldstone type nano titanium dioxide. The rest is the same as in Example 1.
[0089] Example 16
[0090] The difference from Example 1 is that in this example, copper chloride solution is used in step S1, and ammonium persulfate is used as the initiator; the rest is the same as in Example 1.
[0091] Comparative Example 1
[0092] The composite antibacterial finishing agent prepared according to Example 1 disclosed in the specification of patent 202211733862.6 was used as a comparative antibacterial agent.
[0093] Comparative Example 2
[0094] The difference from Example 1 is that in step S1 of this comparative example, no copper ion salt solution is added; the rest is the same as in Example 1.
[0095] Comparative Example 3
[0096] The difference from Example 1 is that in step S2 of this comparative example, nano-titanium dioxide is not added, while the rest is the same as in Example 1.
[0097] Comparative Example 4
[0098] The difference from Example 1 is that in step S1 of this comparative example, no copper ion salt solution is added, and in step S2, no nano titanium dioxide is added; the rest is the same as in Example 1.
[0099] Comparative Example 5
[0100] The difference from Example 1 is that step S1 is omitted, and the copper ion salt solution is directly used as mixture A, while the rest is the same as in Example 1.
[0101] Experimental Example 1
[0102] The antibacterial agents prepared in Examples 1-16, the antibacterial agents prepared in Comparative Examples 2-5, and the antibacterial finishing agent of Comparative Example 1 were taken in equal volumes and placed in different containers. A whole piece of cotton fabric was taken and randomly cut into several pieces of the same area, divided into 21 groups, with the same number of pieces in each group. The 21 groups of fabric pieces were placed in containers containing antibacterial agents, soaked at room temperature for 1 hour, and then dried to obtain antibacterial fabric samples.
[0103] 1. Antibacterial performance test
[0104] The antibacterial properties were tested according to GB / T20944.3-2008, specifically using Escherichia coli (ATCC25922), and the inhibition rate was used as the measure. The inhibition rate was the average of the three fabric samples, and the results are shown in Table 1.
[0105] Table 1. Antibacterial rate of fabrics (%)
[0106] Before washing Wash 10 times Wash 50 times Washed 50 times with water and then exposed to ultraviolet light for 2 hours. Example 1 99.62 99.56 88.63 88.52 Example 2 99.56 99.31 87.36 87.01 Example 3 99.72 99.48 88.46 88.03 Example 4 99.61 99.01 88.35 87.98 Example 5 99.89 99.53 99.02 89.02 Example 6 99.68 99.45 89.88 88.78 Example 7 99.63 99.56 92.31 91.12 Example 8 99.79 99.36 87.78 87.21 Example 9 99.56 99.12 88.02 87.56 Example 10 99.83 99.31 88.63 88.14 Example 11 99.64 99.17 88.21 87.82 Example 12 99.56 99.21 87.98 87.14 Example 13 99.76 99.13 88.34 87.98 Example 14 99.81 99.11 88.25 87.96 Example 15 99.58 99.21 88.45 88.01 Example 16 99.52 99.09 88.11 87.85 Comparative Example 1 98.35 88.21 65.32 30.41 Comparative Example 2 93.23 90.21 80.38 78.25 Comparative Example 3 98.63 93.21 80.21 41.23 Comparative Example 4 93.15 90.13 78.32 52.31 Comparative Example 5 98.45 87.36 60.12 55.18
[0107] As can be seen from Table 1 above, the antibacterial rate of cotton fabrics before washing can reach over 99%, demonstrating excellent antibacterial effects. After multiple washes, the antibacterial rate of the cotton fabrics corresponding to Examples 1-16 decreased, but still remained above 80%. During the washing process, some antibacterial agents will be shed, leading to a decrease in the antibacterial rate. Secondly, the halogen atoms in the antibacterial agent will be consumed as the antibacterial time increases, which will also lead to a decrease in the antibacterial rate of the fabric.
[0108] Specifically, in Examples 5-7, hydroxyl groups and other metal ions were added to the antibacterial agent, which has a stronger binding ability with cotton fabric than the antibacterial agents in other examples. Therefore, the antibacterial rate of the cotton fabrics corresponding to Examples 5-7 is slightly higher than that of other examples after multiple washes. Among them, the cotton fabric of Example 7 can still achieve an antibacterial rate of over 90% after 50 washes. It can be seen that the antibacterial effect of the fabric corresponding to Example 7 is long-lasting, the binding force between the antibacterial agent and the fabric is strong, and the antibacterial agent is not easy to fall off.
[0109] After washing the above fabrics 50 times, they were then irradiated with ultraviolet light for 2 hours. The antibacterial effect of each fabric was then tested. As can be seen from Table 1, the antibacterial rate of the cotton fabrics in Examples 1-16 was not significantly different from that before irradiation after 2 hours of ultraviolet light irradiation. However, the antibacterial rate of Comparative Example 1.3.4 decreased significantly. The reason for this is that Comparative Example 1.3.4 does not contain titanium dioxide, and the N-Cl in the antibacterial agent is easily broken, leading to a sharp decrease in the antibacterial effect.
[0110] The antibacterial agent in Comparative Example 1 had fewer types of antibacterial substances, and its antibacterial rate decreased significantly after multiple washes.
[0111] 2. Antibacterial agent regeneration performance test
[0112] Cotton fabric that had undergone 50 washes and 2 hours of UV irradiation was soaked in a 0.5% sodium hypochlorite solution for 30 minutes, dried, and then tested for its antibacterial rate (antibacterial rate 1) using the same method. A separate piece of fabric from the same material was then immersed in a 1×10⁻⁶ sodium hypochlorite solution. 5 The fabric was placed in a CFU / ml E. coli suspension for 30 min, then immersed in sterile physiological saline for 30 s to wash out the bacteria. This process was repeated several times until the antibacterial rate of the fabric was less than 50%. The fabric was then immersed in a 0.5% sodium hypochlorite solution for 1 h and dried. The antibacterial rate of the cotton fabric was then tested using the same method (antibacterial rate 2). The results are shown in Table 2.
[0113] Table 2 Antimicrobial agent regeneration performance test
[0114]
[0115]
[0116] As can be seen from Table 2 above, after two regeneration methods, the antibacterial rate of the antibacterial fabrics in Examples 1-16 can reach the antibacterial rate before use (before washing in Table 1). It can be seen that the antibacterial agent provided in this application has a good regeneration effect.
[0117] 3. Antibacterial duration test
[0118] Using the above method, the number of times the fabric patch needed to be repeatedly soaked in the E. coli suspension when the antibacterial rate was less than 50% was counted. The number of times was the average of 3 fabric patches. The results are shown in Table 3.
[0119] Table 3. Statistics on antibacterial duration
[0120]
[0121]
[0122] By repeatedly immersing the fabric in E. coli, the condition of cotton fabric being loaded with bacteria during use was simulated. The number of immersions was used to reflect the antibacterial efficacy, that is, the amount of E. coli that the antibacterial agent could kill. As can be seen from Table 3, the antibacterial agents in Examples 1-16 have a long antibacterial efficacy.
[0123] The embodiments described above are some, but not all, embodiments of the present invention. The detailed description of the embodiments of the present invention is not intended to limit the scope of the claimed invention, but merely to illustrate selected embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.
Claims
1. A method for preparing a long-acting antibacterial agent, characterized in that, Includes the following steps: S1: Mix chitosan with an aqueous acetic acid solution and stir at 50-60℃ to dissolve the chitosan; then add 2,3-epoxypropyltrimethylammonium chloride. After the reaction is complete, add a copper ion salt solution to the system, stir evenly, and adjust the pH value to 5-6 to obtain mixture A. S2: Disperse nano-titanium dioxide in an aqueous ethanol solution and add γ-methacryloyloxypropyltrimethoxysilane. Alkane, heat and stir; then add haloamine precursor compound to the system to obtain mixture B; S3: Mix the mixture A prepared in step S1 with the mixture B prepared in step S2, stir evenly, add the initiator, and disperse by ultrasonication; then add sodium hypochlorite solution, disperse by ultrasonication at 30-40℃ and stir for 8-10 hours to obtain the long-acting antibacterial agent; In step S2, the preparation method of the nano-titanium dioxide includes the following steps: dissolving tetraisopropyl titanate and titanate coupling agent in dichloromethane, stirring evenly, then adding an aqueous solution of sodium dodecyl sulfonate and hexadecyltrimethylammonium chloride, stirring at high speed, then adding an aqueous solution of tetramethylguanidine, adjusting the pH value to 7-8, drying, and calcining. In step S1, the mass ratio of chitosan to 2,3-epoxypropyltrimethylammonium chloride is 1:5-8; In step S2, the mass ratio of nano-titanium dioxide to γ-methacryloyloxypropyltrimethoxysilane is 1:30-40, and the mass ratio of nano-titanium dioxide to haloamine precursor compound is 1:4-5.
2. The method for preparing the long-acting antibacterial agent according to claim 1, characterized in that, In step S3, polyvinyl alcohol solution is added first, and after stirring evenly, sodium hypochlorite solution is added.
3. The method for preparing the long-acting antibacterial agent according to claim 1, characterized in that, In step S1, after adding copper ion salt solution and stirring evenly, aluminum chloride aqueous solution is added, ultrasonically dispersed at 50-60℃, and then allowed to stand.
4. The method for preparing the long-acting antibacterial agent according to claim 3, characterized in that, The mass of copper ions in the copper ion salt solution: the mass of aluminum ions in the aluminum chloride aqueous solution = 1:(0.5-1).
5. The method for preparing the long-acting antibacterial agent according to claim 1, characterized in that, The haloamine precursor compound is one or more of 3-allyl-5,5-dimethylhydantoin, 1-allylhydantoin, and 3-(4'-vinylbenzyl)-5,5-dimethylhydantoin.
6. The method for preparing the long-acting antibacterial agent according to claim 1, characterized in that, The initiator is persulfate. One or more of sodium, potassium persulfate, and ammonium persulfate; the copper ion salt is one or more of copper nitrate, copper sulfate, and copper chloride.
7. A long-acting antibacterial agent, characterized in that: It is prepared by the method of any one of claims 1-6 for preparing a long-acting antibacterial agent.
Citation Information
Patent Citations
A method for preparing a betaine-haloamine compound dual antibacterial textile
CN112012012B
Graphene and quaternary ammonium salt-containing textile antibacterial agent and preparation method thereof
CN116084169A
Quaternization hadegen amide modified chitosan and method for preparing antibacterial cotton fabric
CN104628888A
Functionalized titanium dioxide antibacterial hydrogel and preparation method thereof