A kind of ultraviolet curing nanoimprint adhesive and preparation method thereof

By improving the preparation process of ultraviolet nanoimprint photoresist and adding components such as modified polyurethane resin and nano-silica aerosol, the problems of unclear patterns and insufficient release properties of existing photoresists have been solved, achieving high-resolution ultraviolet nanoimprint effects with excellent release properties.

CN117539125BActive Publication Date: 2024-11-08GERMANLITHO CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311535515.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-17
Publication Date
2024-11-08
Estimated Expiration
2043-11-17

AI Technical Summary

Technical Problem

Existing UV nanoimprint photoresists exhibit unclear patterns, insufficient release properties, and poor etching resistance during UV exposure experiments, affecting pattern transfer quality and production efficiency.

Method used

By improving the preparation process and adding modified polyurethane resin, nano-silica aerosol, and specific surfactants, a UV-curable nanoimprint liner was prepared. The liner includes components such as ethylene glycol monoisopropyl ether, reactive diluent hexanediol diacrylate, methyl acrylate, and UV photoinitiator 2,2-diethoxyacetophenone. The viscosity and rheological properties were optimized, and the curing rate and release properties of the photoresist were improved.

Benefits of technology

It achieves high-resolution nanoimprinted patterns, excellent demolding performance and etching resistance, improves the pattern quality and production efficiency of photoresist, and is suitable for the field of ultraviolet nanoimprinting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004554851000000121
    Figure BDA0004554851000000121
  • Figure BDA0004554851000000131
    Figure BDA0004554851000000131
Patent Text Reader

Abstract

The present invention relates to a UV-curable nano-imprint adhesive and a preparation method thereof. The UV-curable nano-imprint adhesive comprises the following components, in parts by weight: 5-20 parts of resin, 5-10 parts of modified polyurethane resin, 1-5 parts of UV initiator, 1-3 parts of polyacrylamide, 1-3 parts of nano-silicon dioxide aerosol, 30-50 parts of ethylene glycol monoisopropyl ether, 10-15 parts of active diluent, 10-20 parts of surfactant, and 5-10 parts of stabilizer. The present invention uses cationic surfactant octadecyl trimethyl ammonium bromide in combination with polyacrylamide, and the prepared nano-imprint adhesive is a nano-imprint adhesive with low surface energy, good filling property, fast curing speed, etching resistance, smooth demoulding, template protection, and the ability to prepare high-resolution nano patterns, while the addition of octadecyl trimethyl ammonium bromide alone only solves the problems of low surface energy and good demoulding property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photoresists, and in particular to an ultraviolet-cured nanoimprint adhesive and a preparation method thereof. Background Art

[0002] Nano-imprint lithography (NIL) is a pattern transfer technology that transfers the characteristic pattern with nanostructure on the template to the substrate in proportion under certain process conditions. Nano-imprint lithography has high resolution, ultra-low cost and high productivity, strong competitiveness and broad development prospects, and is considered to be one of the most promising nano-manufacturing technologies today. Nano-imprint lithography mainly includes hot embossing (HEL), ultraviolet embossing (UV-NIL) and micro-contact printing (HCP) embossing. The basic principle of the process is basically the same, that is, a template with a nano-graphic structure is first produced through conventional microelectronic processes such as electron beam exposure and dry etching. During imprinting, a layer of photoresist is first coated on the surface of the substrate (silicon, quartz glass, etc.). When the photoresist has appropriate fluidity, the template is physically in contact with the substrate surface and the resist is filled with the concave and convex pattern of the template (i.e., imprinting): then the photoresist is cured by ultraviolet exposure or heating, and the pattern on the template is copied to the resist after demolding. Finally, the pattern on the resist is transferred to the substrate through an etching process to form the required nano-graphic structure on the substrate, thus completing the entire nanoimprint process. UV nanoimprint lithography is an imprint lithography technology that uses ultraviolet light to cure polymers at room temperature and low pressure. Since UV nanoimprint lithography uses ultraviolet light for exposure and curing, the template material of UV-NIL must be transparent to ultraviolet light. Basically, quartz material is used as the imprint template, and then a layer of low-viscosity, UV-sensitive liquid photoresist component is coated on the silicon substrate. The template is pressed into the photoresist layer and exposed to ultraviolet light to cause the photoresist to undergo a photocuring reaction. The mold is then demolded, and then the excess photoresist remaining on the substrate is removed by etching methods such as plasma etching. This completes the entire UV nanoimprint lithography process.

[0003] In the process of ultraviolet nanoimprint lithography, photoresist must participate in the ultraviolet photopolymerization curing process. Due to its imprinting process, the formation of the photoresist surface pattern is formed by a template with a convex and concave surface structure. The factors affecting the accuracy of pattern replication are mainly the hardness and viscosity of the photoresist system, and its production efficiency is mainly affected by the curing rate. In order to obtain high-quality patterns and reduce the shortcomings such as pattern defects caused by imprint debonding, it is necessary to ensure that the photoresist has good adhesion to the substrate. In order to obtain high-quality and accurate replicated patterns, it is necessary to ensure that the photoresist has good rheological properties and plasticity. Before and after curing, the hardness of the photoresist changes significantly, from a low hardness in the liquid state to a larger strength after curing. Low-hardness liquid photoresist is conducive to completing imprinting under low pressure, while high-hardness cured photoresist can effectively prevent the fine structure of the pattern from brittle fracture during demolding. Efficient curing will inevitably bring high-efficiency production benefits. Therefore, improving the curing rate is also important for the performance of the photoresist. UV nanoimprinting has developed to date, especially the step-by-step technology and UV nanoimprinting technology combined to form a step-by-step flash UV nanoimprinting that has solved the problem of photoresist curing rate. For the mechanical contact of the UV nanoimprinting process, to avoid the debonding phenomenon between the photoresist and the substrate, a strong bonding force is inevitably required. In order to ensure smooth demolding after the imprinting is completed, it is necessary for the photoresist and the template to have a lower bonding force. In the commonly used photoresist system, the use of pure organic materials with a carbon-oxygen main chain with high surface energy can achieve the purpose of having a strong bonding force with the substrate, but its strong adhesion to the template will cause defects in the imprinted pattern and even damage the template. The use of silicon-containing and fluorine-containing materials with low surface energy can achieve the purpose of smooth demolding, but its low bonding force with the substrate will cause debonding. Combining the characteristics of these two types of materials, adding materials containing carbon-oxygen groups and silicon-oxygen or fluorocarbon groups to the photoresist system can solve these defects and shortcomings of the photoresist. In the usual imprinting process, photoresist is mainly used as a pattern transfer medium. The transfer of photoresist patterns to the substrate is achieved through ion etching. Therefore, to ensure the quality of the transferred patterns, the photoresist is naturally required to have a certain degree of etching resistance and etching selectivity. Generally speaking, organic materials containing silicon have a strong etching resistance due to the high bond energy of silicon-oxygen bonds.

[0004] CN113156765B discloses a photoresist for ultraviolet nanoimprinting and its preparation method and application. The invented photoresist can be used for ultraviolet nanoimprinting, and contains a photopolymerizable disulfide compound that can reduce the volume shrinkage during photopolymerization and impart polymer degradation characteristics, a second photopolymerizable monomer and a photoinitiator. The photopolymerizable disulfide compound in the invented photoresist composition can significantly reduce the volume shrinkage of the photoresist caused by photopolymerization during ultraviolet nanoimprinting, providing excellent ultraviolet nanoimprinting pattern quality; and after ultraviolet light curing, it can be degraded under reducing conditions, which is convenient for cleaning the imprinting template; in addition, the photoresist has low viscosity, which is convenient for imprinting process operation, and the formed polymer film has good physical and mechanical properties. However, the disadvantage is that the stripes displayed by the photoresist prepared by the invention in the ultraviolet exposure experiment are not very clear and the width is not very ideal.

[0005] CN105242493A discloses a UV-curable nanoimprint photoresist and a preparation method thereof. The invention relates to a UV-curable nanoimprint photoresist and a preparation method thereof, wherein the photoresist comprises: 5%-20% epoxy acrylate, 1%-5% UV initiator, 30%-70% ethylene glycol monoisopropyl ether, 10%-15% reactive diluent, 10%-20% surfactant, 5%-10% organosilicon hybrid material, and 0.5%-2% other trace additives. In the absence of UV light, ethylene glycol monoisopropyl ether is first added to the reaction kettle, and then reactive diluent and epoxy acrylate are added under stirring at 80 rpm, and UV initiator is added after 3 minutes, and surfactant, organosilicon hybrid material and trace additive are added after complete dissolution. After 5 minutes, the finished product is obtained by filtering with a 2000-mesh filter. The finished product is transparent and uniform, has good storage performance, and has low viscosity. The silicon hybrid material effectively ensures its anti-etching performance and can obtain high-resolution nano patterns. The disadvantage is that the demoulding property of the nano photoresist prepared by the invention is not very good, which needs to be improved.

[0006] The present invention prepares ultraviolet-cured nanoimprint photoresist with higher resolution and better demoulding property by improving the preparation process and adding new preparation raw materials. Summary of the invention

[0007] The present invention provides a UV-curable nanoimprint adhesive, and the preparation steps are as follows, in parts by weight:

[0008] S1, under the production condition of completely filtering out ultraviolet light, first add 30-50 parts of ethylene glycol monoisopropyl ether and stir at a stirring speed of 80-120r / min for 3-5min;

[0009] S2, while S1 is being stirred, continues to add 10-15 parts of active diluent hexanediol diacrylate, 5-20 parts of resin, and 5-10 parts of modified polyurethane resin, and continues to stir for 3-5 minutes. After being evenly dispersed, continues to add 1-5 parts of ultraviolet light initiator until the light initiator is completely dissolved;

[0010] S3 continues to add 10-20 parts of surfactant, 1-3 parts of polyacrylamide, 1-3 parts of nano-silicon dioxide aerosol and 5-10 parts of stabilizer to S2, and after uniform dispersion, filter with a 0.2-0.4 μm filter membrane to obtain the ultraviolet-cured nano-imprint adhesive of the present invention.

[0011] The resin is at least one of a thermoplastic resin and a photocurable resin; more preferably, the resin is a photocurable resin.

[0012] The thermoplastic resin is at least one of polymethyl methacrylate, polystyrene, polycarbonate and silicone material;

[0013] The photocurable resin is at least one of acrylate, methyl acrylate, and epoxy resin vinyl ether; more preferably, the photocurable resin is methyl acrylate.

[0014] The preparation method of the modified polyurethane resin is as follows, in parts by weight:

[0015] X1 heats the aqueous dispersion of ferrous sulfide and graphite fluoride to 80-100°C and stirs for 2 hours at a stirring speed of 300-400 r / min;

[0016] X2 continues to add 5 to 10 parts of waterborne polyurethane acrylate, and after it is evenly dispersed, the mixed solution is heated to 40 to 60° C. and, under ventilation conditions, waits until the water content evaporates to 20 to 30 wt %.

[0017] The ultraviolet light initiator is at least one of 2-phenylbenzyl-2-dimethylamine-1-(4-morpholinobenzylphenyl)butanone, 2,2-diethoxyacetophenone, 1-hydroxycyclohexylacetophenone, p-isopropylphenyl-2-hydroxydimethylacetone-1, benzophenone, 2-chlorothioxanthone, 4-phenylbenzophenone, 2,4-dimethylthioxanthone, 9,10-phenanthrenequinone, and dimethylamino-p-oxazolidinone; more preferably, the ultraviolet light initiator is 2,2-diethoxyacetophenone.

[0018] The present invention selects ethylene glycol monoisopropyl ether as the solvent, and the solvent has good compatibility with the resin selected by the present invention.

[0019] The particle size of the nano-silicon dioxide aerosol is 40 to 60 nm; more preferably, the particle size of the nano-silicon dioxide aerosol is 50 nm.

[0020] The surfactant is at least one of ethanolamine, polyetheramine D230, polyetheramine D2000, dodecyltrimethylammonium bromide, tetradecyltrimethylammonium bromide, hexadecyltrimethylammonium bromide and octadecyltrimethylammonium bromide; more preferably, the surfactant is octadecyltrimethylammonium bromide.

[0021] The stabilizer is at least one of benzophenone, benzotriazole, salicylic acid aromatic ester, and benzoate stabilizers; more preferably, the stabilizer is a benzotriazole stabilizer; the benzotriazole stabilizer is 2-[2-hydroxy-3-tert-butyl-5-(3-methyl propionate)phenyl]-2H-benzotriazole.

[0022] The UV-curable nanoimprint adhesive of the present invention can obtain a nanoimprint pattern of less than 50 nm; more preferably, the UV-curable nanoimprint adhesive of the present invention can obtain a nanoimprint pattern of 30 nm.

[0023] The UV-curable nanoimprint adhesive of the present invention is used in 200-260nm and 180-190nm nanoimprinting; more preferably, the UV-curable nanoimprint adhesive of the present invention is used in 254nm and 185nm nanoimprinting.

[0024] The functions of the main raw materials in the present invention are introduced as follows:

[0025] Methyl acrylate: 1. It can be used as the main component of nanoimprint glue, together with other monomers and polymers, to form a film with a specific pattern and size through a UV curing reaction; 2. Methyl acrylate is a transparent, colorless, easy-flowing liquid with a strong pungent odor; 3. It has good chemical stability and thermal stability, and can maintain its properties at high temperatures. These characteristics make it an ideal material for preparing photoresists; 4. During the preparation of UV-curing nanoimprint photoresists, methyl acrylate, together with other monomers and polymers, is irradiated with ultraviolet light to initiate a free radical polymerization reaction. This reaction causes methyl acrylate to cross-link and cure with other components to form a film with a specific pattern.

[0026] In general, resin methyl acrylate plays a key role in the preparation of UV-curable nanoimprint adhesives. Its chemical stability and thermal stability make it an ideal material for the preparation of nanoimprint adhesives, while its easy flow properties facilitate the operation of nanoimprint adhesives during the preparation process.

[0027] Modified polyurethane resin: 1. Modified polyurethane resin is made by introducing modifiers or additives into polyurethane resin. These modifiers can be polymers, fillers, flame retardants, etc. By adding these ingredients, modified polyurethane resin can obtain different properties and characteristics, such as enhanced strength, high temperature resistance, chemical corrosion resistance, etc.; 2. In the preparation process of UV-curable nanoimprint adhesive, modified polyurethane resin can be used as one of the main components of nanoimprint adhesive, together with other monomers and polymers, to form a film with a specific pattern and size through UV curing reaction; 3. The flexibility and adhesion of modified polyurethane resin make it play an important role in photoresist, and it also has good compatibility and impact resistance; 4. By adjusting the formula and proportion of modified polyurethane resin, the performance of nanoimprint adhesive can be further optimized, such as improving adhesion, reducing curing temperature, increasing curing speed, etc.; 5. In addition, modified polyurethane resin can also be used as an additive and used with other materials to improve the overall performance of nanoimprint adhesive.

[0028] In the present invention, the effect of adding graphite fluoride directly is not as good as that of adding graphite fluoride dispersed in modified polyurethane.

[0029] In conclusion, modified polyurethane resin plays a key role in the preparation of UV-curable nanoimprint adhesives. Its properties such as flexibility, adhesion and compatibility are of great significance for improving the performance of nanoimprint adhesives and meeting different application requirements.

[0030] UV photoinitiator 2,2-diethoxyacetophenone: 1. The mechanism of action of UV photoinitiator 2,2-diethoxyacetophenone in the preparation of UV-curable nanoimprint adhesive is that it will produce free radicals under the irradiation of ultraviolet light, thereby initiating a polymerization reaction. Specifically, when 2,2-diethoxyacetophenone is irradiated by ultraviolet light, its molecular structure will change and produce free radicals. These free radicals are highly active and can react with other components in the nanoimprint adhesive to form a cross-linked network structure. This reaction process is usually referred to as "curing" or "cross-linking"; 2. In the preparation process of UV-curable nanoimprint adhesive, the role of 2,2-diethoxyacetophenone as an initiator is to control the speed and degree of the polymerization reaction. By adjusting the amount of initiator and the irradiation time of ultraviolet light, the cross-linking degree and curing speed of the nanoimprint adhesive can be controlled; 3. In addition, the solubility and chemical stability of 2,2-diethoxyacetophenone also affect its role in the preparation of UV-curable nanoimprint adhesive. It needs to be compatible with other monomers and polymers to achieve good dispersion and mixing. At the same time, its chemical stability also needs to be high enough to avoid degradation or deterioration during preparation and use.

[0031] In summary, the role of the UV photoinitiator 2,2-diethoxyacetophenone in the preparation of UV-curable nanoimprint adhesive is to initiate the polymerization reaction by generating free radicals, thereby controlling the crosslinking degree and curing speed of the nanoimprint adhesive. At the same time, its solubility and chemical stability also have an important influence on its application effect.

[0032] Nano-silica aerosol: 1. First, nano-silica aerosol has excellent light transmittance, which can effectively improve the light transmittance of nano-imprint adhesive. During the UV curing process, nano-silica aerosol can be evenly dispersed in the nano-imprint adhesive matrix, scattering and refracting ultraviolet light, ensuring the penetration and propagation of light, thereby improving the photocuring efficiency; 2. Secondly, nano-silica aerosol also has good chemical stability and weather resistance, which can effectively improve the durability and stability of nano-imprint adhesive. During the UV curing process, nano-silica aerosol reacts chemically with the photoresist matrix to form chemical bonds, thereby improving the cross-linking density and weather resistance of the nano-imprint adhesive; 3. Finally, nano-silica aerosol can also be used as an enhancer to improve the mechanical properties and wear resistance of nano-imprint adhesive. Because nano-silica aerosol has nano-scale size effect and surface effect, it can effectively improve the mechanical properties of nano-imprint adhesive, improve its hardness, toughness and wear resistance, etc.

[0033] In summary, the mechanism of action of nano-silica aerosol in the preparation of UV-curable nanoimprint adhesive is to improve the light transmittance, chemical stability and mechanical properties of the nanoimprint adhesive to improve its performance, service life, increase product transparency, reduce surface energy and improve demolding effect.

[0034] Solvent ethylene glycol monoisopropyl ether: The role of solvent ethylene glycol monoisopropyl ether in the preparation of UV-curable nanoimprint adhesive is mainly as a solvent and diluent to control the viscosity, rheology and stability of the nanoimprint adhesive. 1. First, ethylene glycol monoisopropyl ether can be used as a solvent to dissolve other components such as monomers, polymers and additives to form a uniform solution. In this process, the chemical properties and polarity characteristics of ethylene glycol monoisopropyl ether play a key role, which is conducive to the mutual dissolution and compatibility of various components; 2. Secondly, ethylene glycol monoisopropyl ether can also be used as a diluent to reduce the viscosity of the nanoimprint adhesive. Viscosity is one of the important parameters of nanoimprint adhesive, which directly affects the fluidity and operability of nanoimprint adhesive. By adding ethylene glycol monoisopropyl ether, the molecular weight and viscosity of each component in the nanoimprint adhesive can be reduced, so that it has better fluidity, which is conducive to the operation and application of the nanoimprint adhesive during preparation and use; 3. Finally, ethylene glycol monoisopropyl ether can also affect the stability and curing speed of the nanoimprint adhesive. During the UV curing process, ethylene glycol monoisopropyl ether will react with other components to promote the curing of the nanoimprint adhesive. At the same time, its dilution effect can also control the curing speed to avoid excessive curing that leads to uneven nanoimprint adhesive.

[0035] In summary, the mechanism of action of the solvent ethylene glycol monoisopropyl ether in the preparation of UV-curable nanoimprint adhesive is to control the viscosity, rheology and stability of the nanoimprint adhesive through dissolution and dilution to achieve good operability and curing effect.

[0036] Reactive diluent hexanediol diacrylate: The role of the reactive diluent hexanediol diacrylate in the preparation of UV-curable nanoimprint adhesive is mainly as a reactive diluent and cross-linking agent to control the viscosity, rheology and curing speed of the nanoimprint adhesive. 1. First, hexanediol diacrylate has the function of a reactive diluent. It can undergo polymerization reaction with other monomers and polymers in the nanoimprint adhesive to form a cross-linked network structure. By adjusting the dosage and ratio of hexanediol diacrylate, the viscosity and rheology of the nanoimprint adhesive can be controlled, so that it has good operability and processability; 2. Secondly, hexanediol diacrylate also has the function of a cross-linking agent. During the UV curing process, hexanediol diacrylate can undergo cross-linking reaction with other monomers and polymers to form a three-dimensional network structure. This cross-linking reaction can enhance the hardness and adhesion of the nanoimprint adhesive and improve its stability and durability; 3. In addition, hexanediol diacrylate can also affect the curing speed and degree of curing of the nanoimprint adhesive. By adjusting the dosage and formulation of hexanediol diacrylate, the curing speed and curing degree of the nanoimprint adhesive can be controlled to meet different application requirements.

[0037] In summary, the mechanism of action of the reactive diluent hexanediol diacrylate in the preparation of UV-curable nanoimprint adhesive is to control the viscosity, rheology and curing speed of the nanoimprint adhesive through the action of reactive dilution and cross-linking agent to achieve good operability and curing effect.

[0038] Stabilizer 2-[2-hydroxy-3-tert-butyl-5-(3-methyl propionate)phenyl]-2H-benzotriazole: The stabilizer 2-[2-hydroxy-3-tert-butyl-5-(3-methyl propionate)phenyl]-2H-benzotriazole is mainly used as a light stabilizer and antioxidant in the preparation of UV-curable nanoimprint adhesive to improve the weather resistance and stability of the nanoimprint adhesive. 1. First, 2-[2-hydroxy-3-tert-butyl-5-(3-methyl propionate)phenyl]-2H-benzotriazole as a light stabilizer can effectively absorb and scatter ultraviolet light to prevent the nanoimprint adhesive from photodegradation or photooxidation under ultraviolet irradiation. This stabilizing effect can protect the molecular structure and chemical bonds of the nanoimprint adhesive, and improve its weather resistance and stability; 2. Secondly, 2-[2-hydroxy-3-tert-butyl-5-(3-methyl propionate)phenyl]-2H-benzotriazole, as an antioxidant, can remove free radicals and oxidation products in the nanoimprint adhesive, and prevent the nanoimprint adhesive from being oxidized and damaged during preparation and use. This antioxidant effect can protect the chemical composition and properties of the nanoimprint adhesive, and improve its stability and durability; 3. In addition, 2-[2-hydroxy-3-tert-butyl-5-(3-methyl propionate)phenyl]-2H-benzotriazole can also affect the curing speed and degree of curing of the nanoimprint adhesive. During the UV curing process, it can undergo cross-linking reactions with other monomers and polymers to form a three-dimensional network structure, thereby improving the hardness and adhesion of the nanoimprint adhesive.

[0039] In summary, the mechanism of action of the stabilizer 2-[2-hydroxy-3-tert-butyl-5-(3-methyl propionate)phenyl]-2H-benzotriazole in the preparation of UV-curable nanoimprint adhesive is to improve the weather resistance and stability of the nanoimprint adhesive through the action of light stabilizer and antioxidant, and at the same time it can also affect the curing speed and degree of curing of the nanoimprint adhesive.

[0040] Beneficial effects of the present invention:

[0041] 1. The UV-curable nanoimprint adhesive of the present invention prepared by a composite surfactant obtained by combining octadecyltrimethylammonium bromide with polyacrylamide not only has good filling performance, fast curing rate, excellent etching resistance, but also has excellent demolding performance.

[0042] 2. The UV-curable nanoimprint adhesive composition prepared by the present invention has excellent demoulding properties due to the introduction of modified polyurethane resin, nano-silica aerosol, and 2-[2-hydroxy-3-tert-butyl-5-(3-methyl propionate)phenyl]-2H-benzotriazole, providing excellent UV nanoimprint pattern quality.

[0043] 3. The UV nanoimprint adhesive composition prepared by the present invention has good degradation performance and demoulding performance under the action of the reducing agent composition after curing, and the nanoimprint adhesive composition has broad application prospects in the field of UV nanoimprint.

[0044] 4. The nanoimprint adhesive prepared by the present invention has low viscosity, is convenient for imprinting process operation, and the formed polymer film has good physical and mechanical properties. DETAILED DESCRIPTION

[0045] In order to further understand the present invention, a UV-curable nanoimprint adhesive and a preparation method thereof provided by the present invention are described in detail below in conjunction with embodiments.

[0046] In the following statements:

[0047] Nano-silica aerosol: Model HSD-5040, particle size 50nm, source: Guangdong Ke Ning Technology Co., Ltd.

[0048] Polyacrylamide: The average molecular weight is 2000.

[0049] Stabilizer 2-[2-hydroxy-3-tert-butyl-5-(3-methyl propionate)phenyl]-2H-benzotriazole: abbreviated as UV-MBHPP, self-made, reference "Wang Baoku. Synthesis of benzotriazole light stabilizers [D]. Tianjin University, 2007."

[0050] Graphite fluoride: CAS number: 51311-17-2, particle size: 50-100 nm, the molar ratio of fluorine to carbon in graphite fluoride is 0.6:1, source: Shanghai Furui Fine Chemical Co., Ltd.

[0051] Waterborne polyurethane acrylate: Model: YT308, source: Shanghai Kaiyin Chemical Co., Ltd.

[0052] Example 1

[0053] A UV-curable nanoimprint adhesive, the preparation steps are as follows:

[0054] S1, under the production condition of completely filtering out ultraviolet light, first add 40.1g of ethylene glycol monoisopropyl ether and stir at a stirring speed of 80r / min for 3min;

[0055] S2, while stirring, continued to add 10.3g of active diluent 1,6-hexanediol diacrylate, 15.2g of methyl acrylate, and 8.0g of modified polyurethane resin, continued to stir for 4min, and after uniform dispersion, continued to add 3.3g of 2,2-diethoxyacetophenone until 2,2-diethoxyacetophenone was completely dissolved;

[0056] S3: 13.5 g of octadecyltrimethylammonium bromide, 2.0 g of polyacrylamide, 3 g of nano-silica aerosol and 6 g of 2-[2-hydroxy-3-tert-butyl-5-(3-methyl propionate)phenyl]-2H-benzotriazole are added, and after being evenly dispersed, the mixture is filtered through a 0.2 μm filter membrane to obtain the ultraviolet-cured nanoimprint adhesive of the present invention.

[0057] The preparation method of the modified polyurethane resin is as follows:

[0058] X1: Heat 0.03g of ferrous sulfide and 0.03g of 27.0g / L graphite fluoride aqueous dispersion to 80°C and stir for 2h at a stirring speed of 300r / min;

[0059] X2 continues to add 8.0g of waterborne polyurethane acrylate, and after it is evenly dispersed, the mixed solution is heated to 45°C and allowed to swell under ventilation conditions until the water content reaches 30wt% under natural ventilation conditions.

[0060] Example 2

[0061] A UV-curable nanoimprint adhesive, the preparation steps are as follows:

[0062] S1, under the production condition of completely filtering out ultraviolet light, first add 40.1g of ethylene glycol monoisopropyl ether and stir at a stirring speed of 80r / min for 3min;

[0063] S2, while S1 is being stirred, continues to add 10.3 g of active diluent 1,6-hexanediol diacrylate, 15.2 g of methyl acrylate, and 8.0 g of modified polyurethane resin, and continues to stir for 4 min. After being evenly dispersed, continues to add 3.3 g of 2,2-diethoxyacetophenone until the photoinitiator is completely dissolved;

[0064] S3 continues to add 15.5 g of octadecyltrimethylammonium bromide, 3 g of nano-silica aerosol and 6 g of 2-[2-hydroxy-3-tert-butyl-5-(3-methyl propionate)phenyl]-2H-benzotriazole to S2, and after uniform dispersion, filter with a 0.2 μm filter membrane to obtain the ultraviolet-cured nanoimprint adhesive of the present invention.

[0065] The preparation method of the modified polyurethane resin is the same as that in Example 1, and will not be repeated here.

[0066] Comparative Example 1

[0067] A UV-curable nanoimprint adhesive, the preparation steps are as follows:

[0068] S1, under the production condition of completely filtering out ultraviolet light, first add 40.1g of ethylene glycol monoisopropyl ether and stir at a stirring speed of 80r / min for 3min;

[0069] S2, while S1 is being stirred, continues to add 10.3 g of active diluent 1,6-hexanediol diacrylate, 15.2 g of methyl acrylate, and 8.0 g of modified polyurethane resin, and continues to stir for 4 min. After being evenly dispersed, continues to add 3.3 g of 2,2-diethoxyacetophenone until the photoinitiator is completely dissolved;

[0070] S3 continues to add 15.5 g of dodecyltrimethylammonium bromide, 3 g of nano-silica aerosol and 6 g of 2-[2-hydroxy-3-tert-butyl-5-(3-methyl propionate)phenyl]-2H-benzotriazole to S2, and after uniform dispersion, filter with a 0.2 μm filter membrane to obtain the ultraviolet-cured nanoimprint adhesive of the present invention.

[0071] The preparation method of the modified polyurethane resin is the same as that in Example 1, and will not be repeated here.

[0072] Test Example 1: UV-cured nanoimprint adhesive resolution test

[0073] First, the silicon wafer was cleaned with a "mixed solvent of sulfuric acid + hydrogen peroxide" with a volume ratio of 2:1 at 100°C for 15 minutes, then cleaned with deionized water, and then wiped with an acetone absorbent cotton ball. Then the silicon wafer was placed on a glue-spinning table (rotation speed of 1800rpm, glue-spinning time of 22s), and the nanoimprint glue Examples 1-2 and Comparative Example 1 prepared in this experiment were coated respectively, and then the above silicon wafer coated with photoresist was placed in a 150°C oven for 70s, and then the silicon wafer was placed under a 193nm deep ultraviolet light exposure machine, a mask was placed on it, and exposure was performed (exposure dose was set to 16mJ·cm -2 ). Then, the exposed silicon wafer was placed in a 1.5% tetramethylammonium hydroxide solution (i.e., as a developer) and, after sufficient development, was quickly taken out and placed in deionized water for fixing. Finally, the fixed silicon wafer was placed at 100°C for 30 minutes, and then a scanning electron microscope (model: S-4800, produced by Hitachi, Japan) was used to test the resolution of the photoresist pattern.

[0074] Table 1 UV-cured nanoimprint glue resolution test results

[0075]

[0076]

[0077] As can be seen from Table 1 above, compared with Example 2, Example 1, i.e., the UV-curable nanoimprint adhesive prepared by combining octadecyltrimethylammonium bromide with polyacrylamide of the present invention, has a higher resolution. The possible reasons are: 1. Surfactant C 18 TAB can effectively reduce the interfacial tension between water and organic solvents, thereby helping nanoparticles to be stably dispersed in water and organic solvents. This helps to prepare nanoparticles with uniform size and shape; 2. PAM is a high molecular polymer with a long chain structure and a large number of polar groups. It can enhance the interaction between nanoparticles and help them to be better dispersed in the photoresist. In addition, PAM can also increase the viscosity and stability of the photoresist, which helps to improve the performance of the photoresist; 3. During the UV curing process, C 18 TAB and PAM may react chemically to form more complex molecular structures. These newly formed molecules may have higher chemical and thermal stability, thereby improving the performance of nanoimprint glue; 4.C 18 The combination of TAB and PAM may change the rheological properties of nanoimprint resists, making them more suitable for nanoimprinting processes, which may help improve the resolution and imaging quality of photoresists.

[0078] In summary, the UV-curable nanoimprint adhesive prepared by the combination of cationic surfactant octadecyltrimethylammonium bromide and polyacrylamide has high resolution, which may be due to their synergistic effect in improving the dispersibility of nanoparticles, enhancing the stability of the nanoimprint adhesive and making it suitable for the operation process.

[0079] Comparison of Example 2 and Comparative Example 1 shows that the resolution of the UV-cured nanoimprint adhesive prepared by the surfactant octadecyl trimethyl ammonium bromide with a longer carbon chain is better. The possible reason is that the cationic surfactant octadecyl trimethyl ammonium bromide (C 18 TAB) and dodecyltrimethylammonium bromide (C 12 TAB) can be used as additives in the preparation of nanoimprint adhesives, but their effects on the performance of nanoimprint adhesives may vary due to their different molecular structures and chemical properties. 18 Compared with TAB, it has a longer carbon chain, which makes it have better dispersibility and wettability in nanoimprint glue. 18 The HLB value (hydrophilic-hydrophobic balance) of TAB is in the range of 17 to 19, indicating that it is a typical surfactant with an amphiphilic structure. 18 TAB exhibits good wetting reversal effect in applications such as oil-based drilling fluids, increasing the tension at the oil-water interface, thereby improving the resolution and demolding properties of nanoimprint adhesives.

[0080] In contrast, dodecyltrimethylammonium bromide (C 12 TAB) has a shorter carbon chain, so its dispersibility and wettability in nanoimprint glue may not be as good as C 18 TAB. In addition, C 12 The low HLB value of TAB indicates that it is highly hydrophilic, which may affect its wetting and dispersion effect at the oil-water interface, thus negatively affecting the resolution and demolding properties of the nanoimprint adhesive.

[0081] Therefore, the nanoimprint glue prepared by cationic surfactant octadecyl trimethyl ammonium bromide has higher resolution and better demolding property than that prepared by dodecyl trimethyl ammonium bromide, which may be attributed to the C 18 TAB has a longer carbon chain and better wetting reversal performance.

[0082] It should be noted that although we have discussed the effects of two cationic surfactants on the performance of nanoimprint adhesives here, in fact, the performance of nanoimprint adhesives is also affected by many factors, such as the formulation of nanoimprint adhesives, manufacturing process, environmental conditions, etc. Therefore, in practical applications, the selection of nanoimprint adhesive additives suitable for specific application scenarios requires consideration of the comprehensive effects of multiple factors.

[0083] Test Example 2: Film-forming and Etching Resistance Test of UV-cured Nanoimprint Glue

[0084] Table 2 Test results of film-forming property and etching resistance of UV-cured nanoimprint adhesive

[0085] Test items Example 1 Example 2 Comparative Example 1 Film forming properties good generally generally Etching rate (nm / s) 1.1 5.1 10.2

[0086] From Table 2 above, it can be seen that the UV-curable nanoimprint adhesive prepared by surfactant octadecyl trimethyl ammonium bromide and polyacrylamide has good film-forming property and etching resistance. The possible reasons are: 1. Synergistic effect: C 18 TAB and PAM may produce synergistic effects in photoresists. 18 As a cationic surfactant, TAB can effectively reduce the interfacial tension between water and organic solvents, helping nanoparticles to be stably dispersed in water and organic solvents. As a high molecular polymer, PAM has a long chain structure and a large number of polar groups, which can enhance the interaction between nanoparticles and help them to be better dispersed in the nanoimprint glue. The combination of these two substances may enable the nanoparticles in the nanoimprint glue to be better arranged and aggregated, forming a denser and more uniform film; 2. Chemical reaction: During the UV curing process, C 18TAB and PAM may react chemically to form a more complex molecular structure. These newly formed molecules may have higher chemical and thermal stability, thereby improving the film-forming and etching resistance of the nanoimprint glue; 3. Interfacial tension and wettability: Octadecyltrimethylammonium bromide is a cationic surfactant that has the effect of reducing interfacial tension and improving wettability. This may enhance the spreading ability of the nanoimprint glue on the surface of the substrate and form a more uniform film. In addition, reducing interfacial tension may also promote the adhesion and arrangement of nanoparticles on the surface of the substrate, further improving the film-forming quality; 4. Etching resistance: The polar groups in PAM may enhance the adhesion between the photoresist and the substrate, thereby improving the etching resistance. In addition, PAM may also affect the etching resistance of the nanoimprint glue by affecting its crosslinking density and hardness. Nanoimprint glues with higher crosslinking density and greater hardness tend to have better etching resistance.

[0087] In summary, the UV-curable nanoimprint adhesive prepared by the combination of surfactant octadecyltrimethylammonium bromide and polyacrylamide has better film-forming properties and etching resistance, which is due to their synergistic effect, chemical reaction, interfacial tension and wettability, and improved etching resistance. However, the specific influencing factors may vary due to differences in nanoimprint adhesive formulation, preparation process, and application. Therefore, in practical applications, it is crucial to select and optimize the appropriate nanoimprint adhesive additive for specific application scenarios.

[0088] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Modifications, replacements, and improvements made within the principles of the present invention should all be included in the protection scope of the present invention.

Claims

1. A method for preparing a UV-curable nanoimprint adhesive, characterized in that: It includes the following components, by weight: S1, under the production condition of completely filtering out ultraviolet light, first add 30-50 parts of ethylene glycol monoisopropyl ether and stir at a stirring speed of 80-120r / min for 3-5min; S2, while S1 is being stirred, continues to add 10-15 parts of active diluent hexanediol diacrylate, 5-20 parts of resin, and 5-10 parts of modified polyurethane resin, and continues to stir for 3-5 minutes. After being evenly dispersed, continues to add 1-5 parts of ultraviolet light initiator until the light initiator is completely dissolved; S3 continues to add 10 to 20 parts of surfactant, 1 to 3 parts of polyacrylamide, 1 to 3 parts of nano-silicon dioxide aerosol and 5 to 10 parts of stabilizer to S2, and after uniform dispersion, filter with a 0.2 to 0.4 μm filter membrane to obtain the ultraviolet-cured nano-imprint adhesive of the present invention; The resin is at least one of a thermoplastic resin and a photocurable resin; The thermoplastic resin is at least one of polymethyl methacrylate, polystyrene, polycarbonate, and silicone materials; the photocurable resin is at least one of acrylate, methyl acrylate, and epoxy resin vinyl ether.

2. The method for preparing a UV-curable nanoimprint adhesive according to claim 1, characterized in that: The preparation method of the modified polyurethane resin is as follows, in parts by weight: X1 heats the aqueous dispersion of ferrous sulfide and graphite fluoride to 80-100°C and stirs for 2 hours at a stirring speed of 300-400 r / min; X2 continues to add 5 to 10 parts of waterborne polyurethane acrylate to X1. After uniform dispersion, the mixed solution is heated to 40 to 60° C. and, under ventilation conditions, the water is evaporated to a content of 20 to 30 wt %.

3. The method for preparing a UV-curable nanoimprint adhesive according to claim 1, characterized in that: The ultraviolet light initiator is at least one of 2-phenylbenzyl-2-dimethylamine-1-(4-morpholinobenzylphenyl)butanone, 2,2-diethoxyacetophenone, 1-hydroxycyclohexylacetophenone, p-isopropylphenyl-2-hydroxydimethylacetone-1, benzophenone, 2-chlorothioxanthone, 4-phenylbenzophenone, 2,4-dimethylthioxanthone, 9,10-phenanthrenequinone, and dimethylamino-p-oxazolidinone; the surfactant is at least one of ethanolamine, polyetheramine D230, polyetheramine D2000, dodecyltrimethylammonium bromide, tetradecyltrimethylammonium bromide, hexadecyltrimethylammonium bromide, and octadecyltrimethylammonium bromide; the stabilizer is at least one of benzophenone, benzotriazole, salicylic acid aromatic ester, and benzoate stabilizer.

4. The method for preparing a UV-curable nanoimprint adhesive according to claim 1, characterized in that: The particle size of the nano silicon dioxide aerosol is 40 to 60 nm.

5. A UV-curable nanoimprint adhesive, characterized in that: Prepared by the method according to any one of claims 1 to 4.

6. Use of the UV-curable nanoimprint adhesive as claimed in claim 5 in nanoimprinting.