Method for resource treatment of lithium iron phosphate waste liquid
Through the multi-step pretreatment, concentration and lithium precipitation treatment process, the problem of low recovery rate of lithium and phosphorus elements in traditional lithium iron phosphate waste liquid treatment is solved, the preparation of high-quality lithium salts and phosphates is achieved, and the phosphoric acid is fully utilized. Iron-lithium waste liquid resources reduce wastewater discharge and operating costs.
Patent Information
- Application Number
- CN202311492621.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-10
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-11-10
AI Technical Summary
The traditional lithium iron phosphate waste liquid treatment process cannot fully utilize the lithium iron phosphate waste liquid as a resource, especially the recovery rate of phosphorus and lithium elements is not high, and the process is complex and costly, making it difficult to obtain high-quality recycling by-products.
Multi-step pretreatment, concentration treatment, lithium precipitation treatment and phosphorus extraction treatment methods are adopted, including filtration, acid-base adjustment, hardness removal, COD removal, reverse osmosis, electrodialysis, lithium precipitation reaction and adsorption and desorption processes to prepare high Quality lithium and phosphate products.
It achieves comprehensive resource utilization of lithium iron phosphate waste liquid, improves the recovery rate of lithium and phosphorus, reduces wastewater discharge, and has the advantages of high resource utilization rate, low operating cost and automatic processing.
Smart Images

Figure CN117550570B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium element extraction, and in particular to a method for resource treatment of lithium iron phosphate waste liquid. Background Art
[0002] Lithium iron phosphate is an important positive electrode material for lithium-ion batteries and is widely used in the field of new energy vehicles. The production process of lithium iron phosphate includes solid-phase method and liquid-phase method. Among them, the carbon thermal reduction method in the solid-phase method is the current mainstream synthesis process. The carbon thermal reduction method uses water-soluble monoammonium phosphate and ferrous sulfate to synthesize iron phosphate, and the mixture containing iron phosphate, lithium carbonate and organic carbon source is subjected to coarse grinding, fine grinding, spray drying, sintering and crushing to obtain lithium iron phosphate. The production raw materials, intermediate products and target products of this method will produce a large amount of phosphorus-containing waste liquid during the washing process. This wastewater will not only cause environmental pollution problems, but also lead to the loss of certain lithium ions in the product. The liquid phase method has higher product consistency and stability, and has been rapidly promoted as production capacity increases. However, a large amount of solvents will be introduced in the production process of the liquid phase method, and its waste liquid treatment requirements are more complicated than those of the solid phase method.
[0003] The key to the treatment of lithium iron phosphate waste liquid is to remove phosphate radicals, organic pollutants and other components. Currently, the commonly used treatment processes mainly include chemical precipitation, adsorption, membrane separation and biological treatment, which can basically solve the environmental pollution problem of lithium iron phosphate waste liquid and some resource recovery problems. However, most traditional lithium iron phosphate waste liquid treatment processes can only recover some components in the wastewater, and the recovery rates of phosphorus and lithium are not high, and lithium iron phosphate waste liquid cannot be fully utilized as a resource. Summary of the invention
[0004] Based on this, it is necessary to provide a method for resource treatment of lithium iron phosphate waste liquid to overcome the problem that most traditional lithium iron phosphate waste liquid treatment processes can only recover some components in the wastewater, the recovery rates of phosphorus and lithium elements are not high, and the lithium iron phosphate waste liquid cannot be fully utilized as a resource.
[0005] The above object of the present invention is achieved through the following technical solutions:
[0006] In a first aspect, the present invention provides a method for recycling lithium iron phosphate waste liquid, comprising the following steps:
[0007] Pre-treating the lithium iron phosphate waste liquid to prepare a pre-treated liquid; wherein the pre-treatment includes filtration treatment, acid-base adjustment treatment, hardness removal treatment and COD removal treatment;
[0008] Concentrating the pre-treated liquid to prepare a concentrated liquid;
[0009] The concentrated solution is subjected to lithium precipitation treatment to prepare a lithium salt product and lithium precipitation waste liquid;
[0010] The lithium precipitation waste liquid is subjected to phosphorus extraction treatment to prepare a phosphate product; wherein the phosphorus extraction treatment includes adsorption treatment and desorption treatment.
[0011] In one embodiment, pre-treating the lithium iron phosphate waste liquid includes the following steps:
[0012] The lithium iron phosphate waste liquid is adjusted to be alkaline by a first acid-base adjustment treatment to prepare a first waste liquid;
[0013] Performing a first hardness removal treatment on the first waste liquid using a calcium and magnesium removal resin to prepare a second waste liquid;
[0014] Performing a first COD removal treatment on the second waste liquid using a COD removal resin to prepare a third waste liquid;
[0015] The phosphate in the third waste liquid is converted into dihydrogen phosphate through a second acid-base adjustment treatment to prepare the pre-treated liquid.
[0016] In one embodiment, one or more of the following conditions are met:
[0017] (1) The pH of the first waste liquid is ≥8;
[0018] (2) The calcium ion content of the second waste liquid is ≤1 mg / L;
[0019] (3) The magnesium ion content of the second waste liquid is ≤1 mg / L;
[0020] (4) The COD content in the third waste liquid is ≤50 mg / L;
[0021] (5) The pH of the pretreatment solution is less than 5.
[0022] In one embodiment, the pretreatment of lithium iron phosphate waste liquid further includes the following steps:
[0023] After the first acid-base adjustment treatment, the lithium iron phosphate waste liquid is subjected to a first filtration treatment to make the suspended matter content of the first waste liquid ≤10 mg / L; and / or,
[0024] After the second acid-base adjustment treatment, the third waste liquid is subjected to a second filtration treatment to make the particle size of the suspended matter in the pre-treated liquid ≤ 0.1 μm.
[0025] In one embodiment, the concentration treatment method includes one or more of reverse osmosis, electrodialysis, nanofiltration and mechanical vapor recompression.
[0026] In one embodiment, the pretreatment liquid is concentrated, comprising the following steps:
[0027] Performing a first concentration treatment on the pre-treated liquid by using the reverse osmosis method to prepare a pre-concentrated liquid;
[0028] The pre-concentrated solution is subjected to a second concentration treatment by using the electrodialysis method to prepare the concentrated solution.
[0029] In one embodiment, before the pre-concentrated solution is subjected to a second concentration treatment by the electrodialysis method, the following steps are also included:
[0030] Performing a second hardness removal treatment on the pre-concentrated liquid using a calcium and magnesium removal resin;
[0031] The pre-concentrated liquid is subjected to a second COD removal treatment using a COD removal resin.
[0032] In one embodiment, the concentrate satisfies one or more of the following conditions:
[0033] (1) The calcium ion content and magnesium ion content of the concentrate are each independently ≤ 1 ppm;
[0034] (2) The COD content of the concentrated liquid is ≤50 mg / L;
[0035] (3) The lithium ion content of the concentrated solution is ≥ 6 g / L;
[0036] (4) The TDS value of the concentrated liquid is ≥100 g / L.
[0037] In one embodiment, the concentrated solution is subjected to lithium precipitation treatment, comprising the following steps:
[0038] The concentrated solution is subjected to a third acid-base adjustment treatment, and a precipitant is added to carry out a lithium precipitation reaction to prepare a mixed slurry;
[0039] The mixed slurry is subjected to solid-liquid separation treatment to prepare the lithium salt product and the lithium precipitation waste liquid.
[0040] In one embodiment, one or more of the following conditions are met:
[0041] (1) The pH of the concentrated solution after the third acid-base adjustment treatment is 8-13;
[0042] (2) The precipitant includes one or more of phosphate, hydrogen phosphate and dihydrogen phosphate;
[0043] (3) The temperature of the lithium precipitation reaction is 90°C to 100°C;
[0044] (4) The solid-liquid separation treatment method includes one or more of a filter press method, a suction filtration method and a centrifugal method.
[0045] In one embodiment, the lithium precipitation waste liquid is subjected to phosphorus extraction treatment, comprising the following steps:
[0046] The lithium precipitation waste liquid is subjected to a fourth acid-base adjustment treatment, and the lithium precipitation waste liquid is subjected to an adsorption treatment using a phosphorus extraction adsorbent to prepare a phosphorus-carrying adsorbent and an adsorbed waste liquid;
[0047] The phosphorus-carrying adsorbent is desorbed by using a desorption liquid to prepare a phosphate solution.
[0048] In one embodiment, one or more of the following conditions are met:
[0049] (1) The pH of the lithium precipitation waste liquid after the fourth acid-base adjustment treatment is 3-4;
[0050] (2) The phosphorus extraction adsorbent comprises a zirconium metal hybrid resin;
[0051] (3) The TP value of the adsorption waste liquid is ≤0.5 mg / L;
[0052] (4) The desorption solution includes one or more of a sodium hydroxide solution, a lithium hydroxide solution and a potassium hydroxide solution;
[0053] (5) The TP value of the phosphate solution is ≥ 6 g / L.
[0054] The present invention has the following beneficial effects:
[0055] The present invention performs a variety of pretreatments on lithium iron phosphate waste liquid in view of its complex composition. Among them, filtration treatment is used to remove suspended solids, acid-base adjustment treatment is used to improve the removal rate of phosphate ions and impurity metal ions, and hardness removal treatment is used to remove Ca 2+ Mg 2+ Impurity metal ions such as COD removal treatment are used to remove organic pollutants, which can effectively avoid the interference of various impurities in lithium iron phosphate waste liquid on lithium precipitation treatment and phosphorus extraction treatment, and reduce the difficulty of separating lithium ions and phosphate. Through concentration treatment, a concentrated solution containing high concentrations of lithium ions and high concentrations of phosphate ions can be obtained; through lithium precipitation treatment, the high concentration of lithium ions in the concentrated solution can be precipitated to prepare high-quality lithium salt products; through phosphorus extraction treatment combined with adsorption treatment and desorption treatment, high-quality phosphate products can be separated from lithium precipitation waste liquid. Therefore, the present invention can obtain high-quality lithium salt products and phosphate products through a variety of pretreatment processes, combined with concentration treatment, lithium precipitation treatment and phosphorus extraction treatment, and make full use of the lithium resources and phosphorus resources in lithium iron phosphate waste liquid, which is conducive to the comprehensive resource utilization of lithium iron phosphate waste liquid. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Figure 1 A schematic diagram of the steps of a method for recycling lithium iron phosphate waste liquid in one embodiment;
[0057] Figure 2 It is a schematic flow chart of a method for resource treatment of lithium iron phosphate waste liquid in one embodiment. DETAILED DESCRIPTION
[0058] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0059] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0060] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0061] Regardless of whether it is a solid phase method or a liquid phase method, a large amount of lithium iron phosphate waste liquid will be generated during the production process of lithium iron phosphate, which mainly contains high concentrations of phosphate ions, sulfate ions, calcium ions, magnesium ions, chemical oxygen demand (COD) and suspended solids (SS). However, the traditional lithium iron phosphate waste liquid treatment process can often only recover part of the components in the waste liquid, for example, recovering sulfate ions and preparing calcium sulfate, recovering ammonia nitrogen and preparing ammonium salts or ammonia gas, which makes it difficult to fully quantify the treatment of this batch of wastewater and the resource utilization rate is low. There are also some waste liquid treatment processes that simply pre-treat the waste liquid and obtain a mixed salt containing ammonium sulfate and ammonium phosphate by evaporation and crystallization. The low-purity mixed salt is difficult to reuse and cannot achieve complete resource utilization.
[0062] There are reports on a method for treating lithium iron phosphate wastewater and recycling resources, which uses an external electrostatic field to drive ion migration through an ion exchange membrane to selectively recover phosphate ions and lithium ions, and recover water resources through multi-effect evaporation; however, the quality of the recovered products of this method is poor, and it requires the use of a mobile electrode capacitor deionization device and a composite electrode material, which has a high investment cost and is not conducive to expanding production. There are reports on a method for treating lithium iron phosphate wastewater, a positive electrode material for lithium batteries, which uses H2O2 oxidation to remove COD, uses a physicochemical precipitation method to remove metal ions, and obtains phosphate salts through tubular tail microfiltration and concentrated evaporation. However, this method completely abandons the effective recovery of lithium resources, the output of precipitated sludge is large, the phosphate product is mixed salt, and the investment and operation and maintenance costs are relatively high.
[0063] It can be seen that the traditional lithium iron phosphate waste liquid treatment process has a low comprehensive recovery rate for phosphorus and lithium elements, and cannot fully utilize lithium iron phosphate waste liquid as a resource. In addition, the traditional process has cumbersome and complicated steps, high investment and operating costs, and usually no way to obtain high-quality recycled by-products, resulting in a low input-output ratio.
[0064] Based on this, the first aspect of the present invention provides a method for resource treatment of lithium iron phosphate waste liquid to solve the problem that most traditional lithium iron phosphate waste liquid treatment processes can only recover some components in the wastewater, the recovery rates of phosphorus and lithium elements are not high, and the lithium iron phosphate waste liquid cannot be fully utilized as a resource.
[0065] In some embodiments, the method for recycling lithium iron phosphate waste liquid comprises the following steps:
[0066] Pre-treating the lithium iron phosphate waste liquid to prepare a pre-treated liquid; wherein the pre-treatment includes filtration treatment, acid-base adjustment treatment, hardness removal treatment and COD removal treatment;
[0067] Concentrating the pre-treated liquid to prepare a concentrated liquid;
[0068] The concentrated solution is subjected to lithium precipitation treatment to prepare lithium salt products and lithium precipitation waste liquid;
[0069] The lithium precipitation waste liquid is subjected to phosphorus extraction treatment to prepare phosphate products; wherein the phosphorus extraction treatment includes adsorption treatment and desorption treatment.
[0070] The present invention performs a variety of pretreatments on lithium iron phosphate waste liquid in view of its complex composition. Among them, filtration treatment is used to remove suspended solids, acid-base adjustment treatment is used to improve the removal rate of phosphate ions and impurity metal ions, and hardness removal treatment is used to remove Ca 2+ Mg 2+Impurity metal ions such as COD removal treatment are used to remove organic pollutants, which can effectively avoid the interference of various impurities in lithium iron phosphate waste liquid on lithium precipitation treatment and phosphorus extraction treatment, and reduce the difficulty of separating lithium ions and phosphate. Through concentration treatment, a concentrated solution containing high concentrations of lithium ions and high concentrations of phosphate ions can be obtained; through lithium precipitation treatment, the high concentration of lithium ions in the concentrated solution can be precipitated to prepare high-quality lithium salt products; through phosphorus extraction treatment combined with adsorption treatment and desorption treatment, high-quality phosphate products can be separated from lithium precipitation waste liquid. Therefore, the present invention can obtain high-quality lithium salt products and phosphate products through a variety of pretreatment processes, combined with concentration treatment, lithium precipitation treatment and phosphorus extraction treatment, and make full use of the lithium resources and phosphorus resources in lithium iron phosphate waste liquid, which is conducive to the comprehensive resource utilization of lithium iron phosphate waste liquid.
[0071] In addition, the method for resource treatment of lithium iron phosphate waste liquid of the present invention will not produce additional physical and chemical sludge, and is conducive to reducing wastewater discharge, with high water reuse efficiency, and has the advantages of high resource utilization rate, good stability, automated processing, and low operating cost. It is conducive to achieving zero-emission treatment of lithium iron phosphate waste liquid and full-quantity, low-energy resource utilization.
[0072] See also Figure 1 and Figure 2 ,in, Figure 1 Schematic diagram of the steps of a method for recycling lithium iron phosphate waste liquid in one embodiment. Figure 2 The figure is a flow chart of a method for recycling lithium iron phosphate waste liquid in one embodiment. The method comprises the following steps:
[0073] S1: pretreating lithium iron phosphate waste liquid to prepare a pretreated liquid.
[0074] In some embodiments, pre-treating the lithium iron phosphate waste liquid comprises the following steps:
[0075] The lithium iron phosphate waste liquid is adjusted to be alkaline through a first acid-base adjustment treatment to prepare a first waste liquid;
[0076] Performing a first hardness removal treatment on the first waste liquid using a calcium and magnesium removal resin to prepare a second waste liquid;
[0077] Performing a first COD removal treatment on the second waste liquid using a COD removal resin to prepare a third waste liquid;
[0078] The phosphate in the third waste liquid is converted into dihydrogen phosphate through the second acid-base adjustment treatment to prepare a pre-treated liquid.
[0079] The above pretreatment process has the following beneficial effects:
[0080] (1) Calcium and magnesium removal resin for Ca 2+Mg 2+ The adsorption selectivity of + Therefore, by the first acid-base adjustment treatment, the lithium iron phosphate waste liquid is adjusted to alkaline, which is beneficial to reduce the adsorption of calcium and magnesium resin to H + The adsorption rate of Ca 2+ Mg 2+ The removal rate and hardness removal effect are significantly improved;
[0081] (2) Thanks to the desorption, regeneration and recycling characteristics of the adsorption resin, the first hardness removal treatment and the first COD removal treatment do not require the addition of additional chemical reagents for precipitation reaction or oxidation reaction. 2+ Mg 2+ The removal rate of COD is high, effectively reducing the impurity content in the pretreatment liquid;
[0082] (3) Through the second acid-base adjustment treatment, the phosphate with lower solubility is converted into dihydrogen phosphate with higher solubility, which can prevent the phosphate concentration from increasing and precipitating during the concentration process, and can avoid the precipitated phosphate from clogging and damaging the concentration equipment. At the same time, it helps to improve the phosphate recovery rate and prevent the waste of phosphorus resources in the waste liquid.
[0083] Optionally, the pH of the first waste liquid is ≥ 8, for example, the pH of the first waste liquid can be 8, 8.1, 8.2, 8.3, 8.4, 8.5, 8.6, 8.7, 8.8, 8.9, 9, 9.1, 9.2, 9.3, 9.4, 9.5, 9.6, 9.7, 9.8, 9.9, 10, 10.5, 11, 11.5, 12, 12.5, 13, 13.5. Further optionally, the pH of the first waste liquid is 8 to 10. Further optionally, the pH of the first waste liquid is 10.
[0084] Optionally, the pH of the pretreatment liquid is less than 5, for example, the pH of the pretreatment liquid may be 5.5, 5, 4.5, 4, 3.5, 3, 2.5, 2, 1.5, or 1; further optionally, the pH of the pretreatment liquid is 2 to 5.
[0085] Optionally, the reagents used in the first acid-base adjustment treatment include one or more of NaOH, Na2CO3, NaHCO3, KOH, K2CO3 and KHCO3.
[0086] Optionally, the reagent used in the first acid-base adjustment treatment includes one or more of HCl, H2SO4 and HNO3.
[0087] Optionally, the calcium-magnesium removal resin meets the following requirements: saturated adsorption capacity is 50 mg / g~75 mg / g, adsorption flow rate is 1 BV / h~10 BV / h, and desorption flow rate is 1 BV / h~4 BV / h.
[0088] Optionally, the COD removal resin meets the following requirements: saturated adsorption capacity is 30 mg / g to 50 mg / g, adsorption flow rate is 1 BV / h to 10 BV / h, and desorption flow rate is 1 BV / h to 4 BV / h.
[0089] Optionally, the calcium ion content of the second waste liquid is ≤1 mg / L, for example, the calcium ion content of the second waste liquid can be 1 mg / L, 0.9 mg / L, 0.8 mg / L, 0.7 mg / L, 0.6 mg / L, 0.5 mg / L, 0.4 mg / L, 0.3 mg / L, 0.2 mg / L, 0.1 mg / L, 0.05 mg / L, 0.01 mg / L. Further optionally, the calcium ion content of the second waste liquid is ≤0.5 mg / L.
[0090] Optionally, the magnesium ion content of the second waste liquid is ≤1 mg / L, for example, the magnesium ion content of the second waste liquid can be 1 mg / L, 0.9 mg / L, 0.8 mg / L, 0.7 mg / L, 0.6 mg / L, 0.5 mg / L, 0.4 mg / L, 0.3 mg / L, 0.2 mg / L, 0.1 mg / L, 0.05 mg / L, 0.01 mg / L. Further optionally, the magnesium ion content of the second waste liquid is ≤0.5 mg / L.
[0091] Optionally, the COD content in the third waste liquid is ≤50 mg / L, for example, the COD content in the third waste liquid can be 50 mg / L, 45 mg / L, 40 mg / L, 35 mg / L, 30 mg / L, 25 mg / L, 20 mg / L, 15 mg / L, 10 mg / L, 5 mg / L, 1 mg / L, 0.5 mg / L, 0.1 mg / L. Further optionally, the COD content in the third waste liquid is ≤25 mg / L.
[0092] In some embodiments, pre-treating the lithium iron phosphate waste liquid further includes the following steps:
[0093] After the first acid-base adjustment treatment, the lithium iron phosphate waste liquid is subjected to a first filtration treatment to make the suspended matter content of the first waste liquid ≤10 mg / L; and / or,
[0094] After the second acid-base adjustment treatment, the third waste liquid is subjected to a second filtration treatment to make the particle size of the suspended matter in the pre-treated liquid ≤ 0.1 μm.
[0095] For example, the suspended matter content of the first waste liquid can be 10 mg / L, 9 mg / L, 8 mg / L, 7 mg / L, 6 mg / L, 5 mg / L, 4 mg / L, 3 mg / L, 2 mg / L, 1 mg / L, 0.5 mg / L, 0.1 mg / L. Further optionally, the suspended matter content of the first waste liquid is ≤5 mg / L.
[0096] For example, the particle size of the suspended matter in the pretreatment liquid can be 100nm, 95nm, 90nm, 85nm, 80nm, 75nm, 70nm, 65nm, 60nm, 55nm, 50nm, 45nm, 40nm, 35nm, 30nm, 25nm, 20nm, 15nm, 10nm, 5nm. Further optionally, the particle size of the suspended matter in the first waste liquid is ≤0.05μm.
[0097] Optionally, the first filtering treatment method includes a sand filtration method and a self-cleaning filtration method, and the equipment of the self-cleaning filtration method is a self-cleaning precision filter.
[0098] Optionally, the second filtering treatment method is a precision filtration method, and the equipment includes a cartridge-type precision filter.
[0099] It can be understood that the sand filter method is a water filtration treatment process using quartz sand, manganese sand or anthracite as filter materials. Quartz sand is mainly used to intercept suspended solids and colloidal substances in water, and manganese sand can remove iron ions in water. The equipment for the first filtration treatment is a self-cleaning precision filter, which has a backwashing function, general filtration accuracy, and a simple backwashing process. In order to improve the filtration accuracy, protect the concentration equipment and save operating costs, a filter element type precision filter can be used for the second filtration treatment after the second acid-base adjustment treatment. It is a security filtration step before the concentration treatment, which can remove suspended solids above 0.1μm. It usually does not have a backwashing function. The filter element is a disposable consumable and the replacement frequency is low.
[0100] Optionally, before the first filtering treatment is performed on the lithium iron phosphate waste liquid, the following steps are also included:
[0101] The lithium iron phosphate waste liquid is homogenized.
[0102] It can be understood that homogenization treatment, also known as slurry treatment, is a treatment process that micronizes and homogenizes the suspended matter in the waste liquid, which plays a role in reducing the particle size of the suspended matter and improving the uniformity of the distribution of the suspended matter.
[0103] S2: Concentrating the pre-treated liquid to prepare a concentrated liquid.
[0104] In some embodiments, the concentration treatment method includes one or more of a reverse osmosis (RO) method, an electrodialysis (ED) method, a nanofiltration (NF) method, and a mechanical vapor recompression (MVR) method.
[0105] Optionally, the concentration treatment method is a reverse osmosis (RO) method and an electrodialysis (ED) method.
[0106] The composite membrane combination process of RO and ED is used for concentration treatment. While obtaining a high-concentration concentrated liquid, it can also improve the water reuse efficiency and reduce the amount of external water discharged by more than 95%.
[0107] In some embodiments, the pre-treatment liquid is concentrated, comprising the following steps:
[0108] Performing a first concentration treatment on the pre-treated liquid by reverse osmosis to prepare a pre-concentrated liquid;
[0109] The pre-concentrated solution is subjected to a second concentration treatment by electrodialysis to prepare a concentrated solution.
[0110] In some embodiments, before the concentrated solution is subjected to a second concentration treatment by electrodialysis, the method further comprises the following steps:
[0111] The pre-concentrated liquid is subjected to a second hardness removal treatment using a calcium and magnesium removal resin;
[0112] The pre-concentrated liquid is subjected to a second COD removal treatment using a COD removal resin.
[0113] The concentration process will not only enrich and concentrate lithium ions and phosphate ions, but also Ca 2+ Mg 2+ Impurities such as COD are also enriched and concentrated, and the impurity concentration is proportional to the adsorption removal efficiency. The impurity concentration in the pre-concentrated liquid obtained by the first concentration treatment is high, and the adsorption removal efficiency is higher than the first hardness removal treatment and the first COD removal treatment, which is beneficial to improve the removal accuracy of impurities and reduce the dryness of impurities to lithium precipitation treatment and phosphorus extraction treatment.
[0114] Optionally, the calcium-magnesium removal resin meets the following requirements: saturated adsorption capacity is 50 mg / g~75 mg / g, adsorption flow rate is 1 BV / h~10 BV / h, and desorption flow rate is 1 BV / h~4 BV / h.
[0115] Optionally, the COD removal resin meets the following requirements: saturated adsorption capacity is 30 mg / g to 50 mg / g, adsorption flow rate is 1 BV / h to 10 BV / h, and desorption flow rate is 1 BV / h to 4 BV / h.
[0116] Optionally, the calcium ion content and magnesium ion content of the concentrate are each independently ≤30ppm. Further optionally, the calcium ion content and magnesium ion content of the concentrate are each independently ≤10ppm
[0117] Optionally, the COD content of the concentrate is ≤300 mg / L, for example, the COD content in the concentrate can be 300 mg / L, 250 mg / L, 200 mg / L, 150 mg / L, 100 mg / L, 50 mg / L, 25 mg / L, 15 mg / L, 10 mg / L, 5 mg / L, 1 mg / L, 0.5 mg / L, 0.1 mg / L. Further optionally, the COD content in the concentrate is ≤150 mg / L.
[0118] Optionally, the lithium ion content of the concentrate is ≥ 6 g / L, for example, the Li + The content can be 6g / L, 7g / L, 8g / L, 9g / L, 10g / L, 11g / L, 12g / L, 13g / L, 14g / L, 15g / L, 16g / L, 17g / L, 18g / L, 19g / L, 20g / L, 25g / L, 30g / L. Further optionally, the Li of the concentrate + Content ≥10g / L.
[0119] Optionally, the TDS value of the concentrate is ≥100 g / L, for example, the total salt content of the concentrate can be 100 g / L, 110 g / L, 120 g / L, 130 g / L, 140 g / L, 150 g / L, 160 g / L, 170 g / L, 180 g / L, 190 g / L, 200 g / L. Further optionally, the total salt content of the concentrate is ≥150 g / L.
[0120] It can be understood that the TDS (Total Dissolved Solids) value, also known as total salt or total salt content, refers to the total content of soluble salt substances in the solution. The size of the TDS value can be used to characterize the purity of the solution or the enrichment of ions.
[0121] Optionally, after the pre-concentrated liquid is subjected to a second concentration treatment by electrodialysis, the method further includes the following steps: desalting the concentrated waste liquid obtained by the second concentration treatment by reverse osmosis to prepare low conductivity water, and making the conductivity of the low conductivity water ≤100 μS / cm.
[0122] Among them, the reverse osmosis method for desalination treatment includes two-stage reverse osmosis and deep reverse osmosis. Through desalination treatment, the impurities in the concentrated waste liquid can be removed to obtain low-salt water that can be reused, thereby reducing the amount of waste water discharged and the water consumption of the entire process, which is conducive to achieving "zero emission" treatment of lithium iron phosphate waste liquid.
[0123] S3: treating the concentrated solution with lithium precipitation to prepare a lithium salt product and lithium precipitation waste liquid;
[0124] In some embodiments, the concentrated solution is subjected to lithium precipitation treatment, comprising the following steps:
[0125] The concentrated solution is subjected to a third acid-base adjustment treatment, and a precipitant is added to carry out a lithium precipitation reaction to prepare a mixed slurry;
[0126] The mixed slurry is subjected to solid-liquid separation to prepare lithium salt products and lithium precipitation waste liquid.
[0127] Optionally, the pH of the concentrated solution after the third acid-base adjustment treatment is 8-13. For example, the pH of the concentrated solution after the third acid-base adjustment treatment may be 8, 8.5, 9, 9.5, 10, 10.5, 11, 11.5, 12, 12.5, or 13. Further optionally, the pH of the concentrated solution after the third acid-base adjustment treatment is 11-13.
[0128] The lithium precipitation reaction is usually carried out under alkaline conditions. As the alkalinity increases, the recovery rate of lithium ions increases. Adjusting the pH of the concentrated solution to the range of 8 to 11 can have the advantages of high lithium ion recovery rate and high cost-effectiveness of lithium precipitation treatment, and is conducive to reducing the difficulty of acid adjustment for subsequent phosphorus extraction treatment; adjusting the pH of the concentrated solution to the range of 11 to 13 can further improve the recovery rate of lithium ions, which is more suitable for lithium precipitation treatment in high-lithium and low-phosphorus systems.
[0129] Optionally, the precipitant includes one or more of phosphate, hydrogen phosphate and dihydrogen phosphate. Further optionally, the precipitant is a phosphate, for example, sodium phosphate and potassium phosphate.
[0130] Among them, the solubility of phosphate is lower than that of hydrogen phosphate and dihydrogen phosphate, and no additional carbonate ions are introduced, which can improve the recovery rate of lithium ions and the purity of lithium salt products.
[0131] Optionally, the molar ratio of phosphate ions in the precipitant to lithium ions in the concentrated solution is (1-1.5):3, for example, the molar ratio of phosphate ions in the precipitant to lithium ions in the concentrated solution may be 1:3, 1.1:3, 1.2:3, 1.3:3, 1.4:3, 1.5:3. Further optionally, the molar ratio of phosphate ions in the precipitant to lithium ions in the concentrated solution is (1.2-1.5):3.
[0132] Optionally, the lithium salt product includes one or more of lithium phosphate, lithium hydrogen phosphate and lithium dihydrogen phosphate. Further optionally, the lithium salt product includes lithium phosphate. In some specific embodiments, the lithium salt product is lithium phosphate ointment.
[0133] Optionally, the temperature of the lithium precipitation reaction is 90° C. to 100° C. For example, the temperature of the lithium precipitation reaction can be 90° C., 91° C., 92° C., 93° C., 94° C., 95° C., 96° C., 97° C., 98° C., 99° C., 100° C. Further optionally, the temperature of the lithium precipitation reaction is 95° C. to 98° C.
[0134] Optionally, the lithium precipitation reaction time is 30min~90min, for example, the lithium precipitation reaction time can be 30min, 35min, 40min, 45min, 50min, 55min, 60min, 65min, 70min, 75min, 80min, 85min, 90min. Further optionally, the lithium precipitation reaction time is 45min~75min.
[0135] Optionally, the solid-liquid separation treatment method includes one or more of a filter press method, a suction filtration method and a centrifugation method. Further optionally, the solid-liquid separation treatment method is a filter press method.
[0136] Among them, the filter press method is a solid-liquid separation process that uses positive pressure to remove water from the mixed slurry; the mixed slurry is placed on the filter cloth of a plate and frame filter press or a belt filter press, and then positive pressure is applied to remove the water from the mixed slurry to achieve the purpose of solid-liquid separation. This method has good solid-liquid separation effect and large processing capacity, but the equipment cost is high and the maintenance cost is also high. It is suitable for large-scale treatment plants.
[0137] Optionally, the lithium salt product includes one or more of lithium phosphate, lithium hydrogen phosphate, lithium dihydrogen phosphate, lithium carbonate and lithium bicarbonate. Further optionally, the lithium salt product is lithium phosphate.
[0138] Optionally, the water content of the lithium salt product is ≤30%, for example, the water content of the lithium salt product may be 30%, 29%, 28%, 27%, 26%, 25%, 24%, 23%, 22%, 21%, 20%, 15%, 10%, 5%, 1%. Further optionally, the water content of the lithium salt product is ≤20%.
[0139] Optionally, the purity of the lithium salt product is ≥65%, for example, the purity of the lithium salt product may be 65%, 70%, 75%, 80%, 85%, 90%, 95%, or 99%.
[0140] Optionally, the lithium ion content of the lithium ion waste liquid is ≤300 mg / L, for example, the lithium ion content of the lithium ion waste liquid can be 300 mg / L, 250 mg / L, 200 mg / L, 150 mg / L, 100 mg / L, 50 mg / L, 25 mg / L, 20 mg / L, 10 mg / L, 5 mg / L, 1 mg / L, 0.1 mg / L. Further optionally, the lithium ion content of the lithium ion waste liquid is ≤150 mg / L.
[0141] Optionally, the lithium ion precipitation recovery rate is ≥90%, and the lithium ion comprehensive recovery rate is ≥80%.
[0142] Among them, the lithium ion precipitation recovery rate is the lithium ion recovery rate in the concentrated solution, and the lithium ion comprehensive recovery rate is the lithium ion recovery rate in the lithium iron phosphate waste liquid. The pretreatment in step S1 and the concentration treatment in step S2 also cause a certain amount of lithium loss, so the lithium ion comprehensive recovery rate is lower than the lithium ion precipitation recovery rate. Usually, the lithium ion content of the lithium iron phosphate waste liquid, the concentrated solution and the lithium precipitation waste liquid can be measured by an analytical method such as the ICP method, and the lithium ion precipitation recovery rate and the lithium ion comprehensive recovery rate can be calculated respectively.
[0143] S4: extracting phosphorus from the lithium precipitation waste liquid to prepare phosphate products.
[0144] In some embodiments, the lithium precipitation waste liquid is subjected to phosphorus extraction treatment, comprising the following steps:
[0145] The lithium precipitation waste liquid is subjected to a fourth acid-base adjustment treatment, and the lithium precipitation waste liquid is subjected to an adsorption treatment using a phosphorus extraction adsorbent to prepare a phosphorus-carrying adsorbent and an adsorbed waste liquid;
[0146] The phosphorus-carrying adsorbent is desorbed by using a desorption liquid to prepare a phosphate solution.
[0147] Optionally, the pH of the lithium precipitation waste liquid after the fourth acid-base adjustment treatment is 3~4, for example, 3, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.
[0148] Optionally, the phosphorus extraction adsorbent comprises a zirconium metal hybrid resin.
[0149] Optionally, the phosphorus extraction adsorbent meets the following requirements: saturated adsorption capacity is 50 mg / g~75 mg / g, adsorption flow rate is 1 BV / h~10 BV / h, and desorption flow rate is 1 BV / h~4 BV / h.
[0150] Optionally, the TP value of the adsorption waste liquid is ≤0.5 mg / L, for example, the TP value of the adsorption waste liquid can be 0.5 mg / L, 0.4 mg / L, 0.3 mg / L, 0.2 mg / L, 0.1 mg / L, 0.08 mg / L, 0.06 mg / L, 0.04 mg / L, 0.02 mg / L, 0.01 mg / L. Further optionally, the TP value of the adsorption waste liquid is ≤0.2 mg / L.
[0151] Understandably, the TP (Total Phosphorus) value is also called the total phosphorus content, which is the phosphorus content measured after the solution sample is digested or oxidized to convert various forms of phosphorus (elemental phosphorus, orthophosphate, condensed phosphate, pyrophosphate, metaphosphate and phosphate combined with organic groups, etc.) into orthophosphate, and is measured in milligrams of phosphorus per liter of solution sample. The TP value of the phosphorus extraction wastewater after phosphorus extraction treatment is less than 0.5mg / L, which meets the secondary standard for sewage treatment.
[0152] Optionally, the desorption solution includes one or more of a sodium hydroxide solution, a lithium hydroxide solution and a potassium hydroxide solution.
[0153] Optionally, the TP value of the phosphate solution is ≥6 g / L, for example, the TP value of the phosphate solution can be 6 g / L, 7 g / L, 8 g / L, 9 g / L, 10 g / L, 15 g / L, 20 g / L, 50 g / L. Further optionally, the TP value of the phosphate solution is ≥10 g / L.
[0154] Optionally, the recovery rate of phosphorus element is ≥99%.
[0155] The TP value of the phosphate solution obtained by phosphorus extraction treatment can reach 6 g / L, and can be used as a precipitant for the lithium precipitation reaction in step S3. The product utilization rate is high, and the amount of added reagents used is reduced, and the operating cost can be further reduced.
[0156] Optionally, after the phosphorus-carrying adsorbent is desorbed by the desorption liquid, the following steps are further included:
[0157] The phosphate solution is subjected to a third concentration treatment by a nanofiltration (NF) method to prepare a phosphate product and an alkaline solution.
[0158] By using a phosphorus-extracting adsorbent to adsorb lithium-precipitated waste liquid, the recovery rate of phosphorus can reach 99%, which is conducive to the full quantitative utilization of phosphorus resources in the waste liquid. At the same time, using alkaline solution as the desorption liquid of the phosphorus-carrying adsorbent, the resulting phosphate solution can be subjected to the third concentration treatment to prepare a high-purity phosphate product and an alkaline solution, and the alkaline solution can be used for the third acid-base adjustment treatment in step S3, reducing the amount of waste liquid discharged and the amount of added reagents used, and achieving the goals of "zero emission" and low energy consumption.
[0159] The present invention is further described in detail below with reference to specific embodiments.
[0160] In the following specific embodiments and comparative examples, the raw materials used, unless otherwise specified, are all commercially available products; the instruments used, unless otherwise specified, are all commercially available products; and the processes used, unless otherwise specified, are all routinely selected by those skilled in the art.
[0161] Among them, the calcium and magnesium removal resin is an aminocarboxylic acid chelating resin selected from Jiangsu Haipu, and the saturated adsorption capacity for calcium and magnesium ions is 50 mg / g.
[0162] The COD removal resin is a hydrophilically modified macroporous polystyrene resin selected from Jiangsu Haipu, and the saturated adsorption capacity of phenol is 30 mg / g.
[0163] The phosphorus extraction adsorbent is a zirconium metal hybrid resin selected from Jiangsu Haipu, and its saturated adsorption capacity for total phosphorus is 21 mg / g.
[0164] Example 1
[0165] The lithium iron phosphate waste liquid of this embodiment comes from the raw material washing water and product washing water when lithium iron phosphate is prepared by a combination of a solid phase method and a liquid phase method, and its component contents are shown in Table 1.
[0166] Table 1. Indicators of lithium iron phosphate waste liquid
[0167]
[0168] (1) Preprocessing:
[0169] Please refer to Table 2. The lithium iron phosphate waste liquid is homogenized to obtain a homogeneous waste liquid. A 2 mol / L NaOH solution is used to perform a first acid-base adjustment treatment to obtain a first waste liquid. The first waste liquid is filtered using sand filtration and a self-cleaning precision filter to make the suspended matter content of the first waste liquid ≤10 mg / L. The first waste liquid is subjected to a first hardness removal treatment using a calcium and magnesium removal resin to obtain a second waste liquid.
[0170] The second waste liquid is subjected to a first COD removal treatment using a COD removal resin to obtain a third waste liquid; a second acid-base adjustment treatment is performed using a 2 mol / L H2SO4 solution to convert phosphate in the third waste liquid into dihydrogen phosphate to obtain a pretreated liquid; a second filtration treatment is performed using a cartridge filter to further remove suspended matter with a particle size > 0.1 μm.
[0171] Table 2. Indices of each solution in step (1)
[0172]
[0173] (2) Concentration treatment:
[0174] Please refer to Table 3. The pre-treated liquid is subjected to a first concentration treatment by a primary RO to obtain a pre-concentrated liquid. The pre-concentrated liquid is subjected to a second hardness removal treatment by using a calcium and magnesium removal resin, and the pre-concentrated liquid is subjected to a second COD removal treatment by using a COD removal resin.
[0175] The pre-concentrated liquid is subjected to a second concentration treatment by ED to obtain a concentrated liquid and a concentrated waste liquid, wherein the TDS value of the concentrated liquid is ≥120g / L; the concentrated waste liquid is desalted by secondary RO and deep RO to obtain low-conductivity water with a conductivity of ≤100μS / cm, which is reused as system water for the waste liquid resource treatment process.
[0176] Table 3. Indices of each solution in step (2)
[0177]
[0178] (3) Lithium precipitation treatment:
[0179] Please refer to Table 4. The concentrate was subjected to a third acid-base adjustment treatment using a 2 mol / L NaOH solution to maintain the pH at 11, and then sodium phosphate solid was gradually added to carry out lithium precipitation reaction. The reaction temperature was 90°C and the reaction time was 60 min. The molar ratio of phosphate ions in the sodium phosphate solid to lithium ions in the concentrate was 1.2:3 to obtain a mixed slurry.
[0180] The mixed slurry is placed in a filter press for solid-liquid separation to obtain lithium phosphate ointment and lithium precipitation waste liquid; wherein the water content of the lithium phosphate ointment is ≤30% and the purity is ≥65%; the Li + Content ≤300mg / L, Li + Recovery rate ≥90%.
[0181] Table 4. Indices of each solution in step (3)
[0182]
[0183] (4) Phosphorus extraction treatment:
[0184] Please refer to Table 5. The lithium precipitation waste liquid is subjected to the fourth acid-base adjustment treatment using a 2 mol / L H2SO4 solution to keep the pH at 3-4. The acidic lithium precipitation waste liquid is subjected to adsorption treatment using a phosphorus extraction adsorbent to prepare a phosphorus-carrying adsorbent and adsorption waste liquid. The phosphorus-carrying adsorbent is subjected to desorption treatment using a 2 mol / L NaOH solution to obtain a sodium phosphate solution and a desorption waste liquid. The sodium phosphate solution is subjected to the third concentration treatment using a nanofiltration method to obtain a sodium phosphate product and an alkaline solution. The alkaline solution can be used for the third acid-base adjustment treatment in step (3) to achieve internal circulation.
[0185] Among them, the TP value of the sodium phosphate solution is ≥6g / L, the TP value of the adsorption waste liquid is ≤0.5mg / L, and the recovery rate of phosphorus element is ≥99%.
[0186] Table 5. Indices of each solution in step (4)
[0187]
[0188] Example 2
[0189] The process parameters of this embodiment are basically the same as those of Embodiment 1, except that in step (3), the pH of the concentrated solution before the lithium precipitation reaction is adjusted to 8.
[0190] Example 3
[0191] The process parameters of this embodiment are basically the same as those of Embodiment 1, except that the calcium ion content of the pretreatment liquid in step (1) is 2 mg / L, the calcium ion content of the concentrated liquid in step (2) is 26 mg / L, and the TDS value is 80 g / L.
[0192] Comparative Example 1
[0193] The process parameters of this embodiment are basically the same as those of Embodiment 1, except that: no hardness removal treatment and COD removal treatment are performed in steps (1) to (2); wherein the calcium ion content of the pretreatment liquid in step (1) is 10 mg / L, and the COD content is 120 mg / L; the calcium ion content of the concentrated liquid in step (2) is 40 mg / L, the COD content is 350 mg / L, the TDS value is 70 g / L, and the lithium ion content is ~4.5 g / L.
[0194] Comparative Example 2
[0195] The process parameters of this embodiment are basically the same as those of Embodiment 1, except that: no hardness removal treatment is performed in steps (1) to (2), wherein the calcium ion content of the pretreatment liquid in step (1) is 10 mg / L; the electrodialysis module cannot be used in the concentration treatment of step (2), the calcium ion content of the concentrated liquid is 50 mg / L, the TDS value is ~80 g / L, the lithium ion content is 5 g / L, and the lithium ion recovery rate is only 75%.
[0196] Comparative Example 3
[0197] The difference between this comparative example and Example 1 is that in step (4), the phosphate is recovered by precipitation method, and the specific steps are as follows:
[0198] The pH of the lithium precipitation waste liquid was adjusted to 7 by 2 mol / L hydrochloric acid. After adding calcium chloride precipitant and reacting for 30 minutes, sodium hydroxide was added to adjust the pH to 10. The phosphate ion removal rate reached 90%. The solid-liquid separation obtained the sludge containing calcium phosphate, which could not be used as a precipitant for lithium precipitation treatment and could not be reused within the system. Therefore, the resource reuse rate was low.
[0199] Test Case
[0200] The treatment effects of lithium iron phosphate waste liquid in Examples 1 to 3 and Comparative Examples 1 to 3 are compared, and the results are shown in Table 6. As can be seen from Table 6, the Li iron phosphate waste liquid treatment method of the present invention is + The recovery rate (i.e., the lithium ion precipitation recovery rate mentioned above) can reach 90%, and the phosphorus recovery rate can reach 99%. High-purity lithium phosphate ointment and sodium phosphate solution can be recovered. The sodium phosphate solution can be reused as a precipitant for lithium precipitation treatment, and can also be further concentrated to obtain high-quality sodium phosphate products. The lithium and phosphorus resources of lithium iron phosphate waste liquid are fully utilized, and the comprehensive resource utilization rate is high.
[0201] Comparative Example 1 did not undergo hardness removal and COD removal treatment, and Comparative Example 2 did not undergo hardness removal treatment. The lithium ion recovery rate and the purity of lithium phosphate ointment were greatly reduced, indicating that the combination of multiple pretreatment processes can reduce the difficulty of lithium extraction, improve the lithium ion recovery rate, and increase the purity of lithium salt products. Comparative Example 3 used precipitation method for phosphorus extraction. The TP value of phosphorus element precipitation waste liquid was only 90%, and the precipitation sludge was calcium phosphate, which could not be used as a precipitant for lithium precipitation treatment. The sludge output was large and difficult to reuse; at the same time, the TP value of the precipitation waste liquid was as high as 600 mg / L, which did not meet the sewage discharge standard and was not suitable for system reuse. Other processes were required for secondary phosphorus extraction. Therefore, this method had low utilization of phosphorus resources, high sewage sludge discharge, and could not achieve full quantitative treatment of lithium iron phosphate waste liquid.
[0202] Table 6. Comparison of lithium iron phosphate wastewater treatment effects
[0203]
[0204] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0205] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims, and the description can be used to interpret the content of the claims.
Claims
1. A method for recycling lithium iron phosphate waste liquid, characterized in that: The following steps are involved: The lithium iron phosphate waste liquid is pretreated to prepare a pretreated liquid, wherein the pretreatment includes filtering treatment, acid-base adjustment treatment, hardness removal treatment and COD removal treatment; the lithium iron phosphate waste liquid is pretreated, comprising the following steps: The lithium iron phosphate waste liquid is adjusted to be alkaline by a first acid-base adjustment treatment to prepare a first waste liquid; Performing a first hardness removal treatment on the first waste liquid using a calcium and magnesium removal resin to prepare a second waste liquid; Performing a first COD removal treatment on the second waste liquid using a COD removal resin to prepare a third waste liquid; The phosphate in the third waste liquid is converted into dihydrogen phosphate by a second acid-base adjustment treatment to prepare the pre-treated liquid; Concentrating the pre-treated liquid to prepare a concentrated liquid; The concentrated solution is subjected to lithium precipitation treatment to prepare a lithium salt product and lithium precipitation waste liquid; The lithium precipitation waste liquid is subjected to phosphorus extraction treatment to prepare a phosphate product; wherein the phosphorus extraction treatment includes adsorption treatment and desorption treatment.
2. The method for recycling lithium iron phosphate waste liquid as claimed in claim 1, characterized in that: One or more of the following conditions are met: (1) The pH of the first waste liquid is ≥8; (2) the calcium ion content of the second waste liquid is ≤1 mg / L; (3) the magnesium ion content of the second waste liquid is ≤1 mg / L; (4) the COD content in the third waste liquid is ≤50 mg / L; (5) The pH of the pretreatment solution is less than 5.
3. The method for recycling lithium iron phosphate waste liquid as claimed in claim 1, characterized in that: The pretreatment of lithium iron phosphate waste liquid also includes the following steps: After the first acid-base adjustment treatment, the lithium iron phosphate waste liquid is subjected to a first filtration treatment to make the suspended matter content of the first waste liquid ≤10 mg / L; and / or, After the second acid-base adjustment treatment, the third waste liquid is subjected to a second filtration treatment to make the particle size of the suspended matter in the pre-treated liquid ≤ 0.1 μm.
4. The method for recycling lithium iron phosphate waste liquid according to any one of claims 1 to 3, characterized in that: The concentration treatment method includes one or more of reverse osmosis, electrodialysis, nanofiltration and mechanical vapor recompression.
5. The method for recycling lithium iron phosphate waste liquid as claimed in claim 4, characterized in that: The pretreatment liquid is concentrated, comprising the following steps: Performing a first concentration treatment on the pre-treated liquid by using the reverse osmosis method to prepare a pre-concentrated liquid; The pre-concentrated solution is subjected to a second concentration treatment by using the electrodialysis method to prepare the concentrated solution.
6. The method for recycling lithium iron phosphate waste liquid as claimed in claim 5, characterized in that: Before the pre-concentrated solution is subjected to a second concentration treatment by the electrodialysis method, the following steps are also included: Performing a second hardness removal treatment on the pre-concentrated liquid using a calcium and magnesium removal resin; The pre-concentrated liquid is subjected to a second COD removal treatment using a COD removal resin.
7. The method for recycling lithium iron phosphate waste liquid as claimed in claim 6, characterized in that: The concentrate meets one or more of the following conditions: (1) The calcium ion content and the magnesium ion content of the concentrated solution are each independently ≤30 ppm; (2) The COD content of the concentrated liquid is ≤300 mg / L; (3) The lithium ion content of the concentrated solution is ≥ 6 g / L; (4) The TDS value of the concentrated solution is ≥100 g / L.
8. The method for recycling lithium iron phosphate waste liquid according to any one of claims 1 to 3 and 5 to 7, characterized in that: The concentrated solution is subjected to lithium precipitation treatment, comprising the following steps: The concentrated solution is subjected to a third acid-base adjustment treatment, and a precipitant is added to carry out a lithium precipitation reaction to prepare a mixed slurry; The mixed slurry is subjected to solid-liquid separation treatment to prepare the lithium salt product and the lithium precipitation waste liquid.
9. The method for recycling lithium iron phosphate waste liquid as claimed in claim 8, characterized in that: One or more of the following conditions are met: (1) The pH of the concentrated solution after the third acid-base adjustment treatment is 8 to 13; (2) the precipitant comprises one or more of phosphate, hydrogen phosphate and dihydrogen phosphate; (3) The temperature of the lithium precipitation reaction is 90° C. to 100° C.; (4) The solid-liquid separation treatment method includes one or more of a filter press method, a suction filtration method and a centrifugal method.
10. The method for recycling lithium iron phosphate waste liquid as claimed in claim 9, characterized in that: The lithium precipitation waste liquid is subjected to phosphorus extraction treatment, comprising the following steps: The lithium precipitation waste liquid is subjected to a fourth acid-base adjustment treatment, and the lithium precipitation waste liquid is subjected to an adsorption treatment using a phosphorus extraction adsorbent to prepare a phosphorus-carrying adsorbent and an adsorbed waste liquid; The phosphorus-carrying adsorbent is desorbed by using a desorption liquid to prepare a phosphate solution.
11. The method for recycling lithium iron phosphate waste liquid as claimed in claim 10, characterized in that: One or more of the following conditions are met: (1) The pH of the lithium precipitation waste liquid after the fourth acid-base adjustment treatment is 3 to 4; (2) The phosphorus extraction adsorbent includes a zirconium metal hybrid resin; (3) The TP value of the adsorption waste liquid is ≤0.5 mg / L; (4) the desorption solution comprises one or more of a sodium hydroxide solution, a lithium hydroxide solution and a potassium hydroxide solution; (5) The TP value of the phosphate solution is ≥6 g / L.
Citation Information
Patent Citations
Method for recovering and preparing battery-grade lithium carbonate and iron phosphate from positive electrode powder of waste lithium iron phosphate battery
CN113912032A
Method for preparing iron powder, lithium phosphate and sodium phosphate from lithium iron phosphate waste
CN115477290A
Treatment method of waste lithium battery leachate
CN115652109A
Method for preparing battery-grade iron phosphate and lithium carbonate from crude lithium phosphate
CN116409769A
Method for preparing lithium carbonate from lithium-containing waste residues and application thereof
CN116835614A