Metallocene polyethylene heat shrinkable film and its composition and preparation method

By using the composition of metallocene polyethylene heat shrinkable film, the problem of insufficient mechanical properties and optical properties of the existing polyethylene heat shrinkable film is solved, better mechanical properties and optical properties are achieved, and it is suitable for the packaging field.

CN117567809BActive Publication Date: 2024-10-29XINJIANG DUSHANZI PETROCHEMICAL CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410061701.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-16
Publication Date
2024-10-29
Estimated Expiration
2044-01-16

AI Technical Summary

Technical Problem

The mechanical properties, thermal shrinkage properties and optical properties of existing polyethylene heat shrinkable films are difficult to meet the requirements of the packaging field.

Method used

A composition using metallocene polyethylene heat shrinkable film, including metallocene polyethylene, octene copolymer linear metallocene polyethylene and linear low density polyethylene as raw materials for the inner layer, middle layer and outer layer, through three-layer co-extrusion Film blowing equipment performs film blowing processing to form heat shrinkable films with excellent mechanical properties, heat shrinkage properties and optical properties.

Benefits of technology

The mechanical properties and optical properties of the heat shrink film are improved, suitable for the packaging field, and the thickness of the product is reduced, while maintaining good heat sealing performance and printing adaptability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117567809B_ABST
    Figure CN117567809B_ABST
Patent Text Reader

Abstract

The present application relates to a metallocene polyethylene heat shrinkable film and a composition and a preparation method thereof, belonging to the technical field of polymer materials; the composition comprises high-density polyethylene, octene copolymer linear metallocene polyethylene, metallocene polyethylene and linear low-density polyethylene; high-density polyethylene, octene copolymer linear metallocene polyethylene, metallocene polyethylene and linear low-density polyethylene are used as components to change the entanglement effect between polyethylene molecular chains, improve the shrinkage rate of long chain branches in the formula during heat shrinkage, and when used in the production of heat shrinkable films, the thickness of the product can be reduced and good mechanical properties can be maintained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polymer materials, and in particular to a metallocene polyethylene heat shrinkable film and a composition and a preparation method thereof. Background Art

[0002] Heat shrink film, commonly known as shrink film, is a film that can shrink significantly after being heated, so it can wrap objects tightly and maintain its shape for a long time. Heat shrink film is designed based on the principle of polymer molecular chain stretching orientation and is formed by rapid cooling and shaping. Its physical principle is: when the plastic raw material is heated and plasticized and extruded into a mother film, the polymer is forcibly stretched in the vertical and horizontal directions between the glass transition temperature and the viscosity flow temperature, so that the polymer molecular chain is oriented along the stretching direction, and then the polymer is rapidly cooled and the molecular orientation is frozen. When the film is reheated to the "thawing" temperature, the stress relaxation caused by molecular movement causes the molecules to return to their original state and shrink. Therefore, heat shrink film is required to have high puncture resistance, good shrinkage and shrinkage stress. It is mainly used for the packaging of bottled beverages and other heavy items, such as collective packaging of alcoholic beverages, cans, and mineral water, and can partially replace carton packaging.

[0003] Conventional heat shrink films mainly include polyvinyl chloride heat shrink films, polyethylene heat shrink films and polyolefin multilayer heat shrink films (POF heat shrink films). Among them, polyvinyl chloride heat shrink films are toxic due to the presence of vinyl chloride monomers. As consumers become more aware of health and environmental protection, their use has been restricted to the food industry. POF heat shrink films are produced by double-bubble method by combining linear low-density polyethylene and copolymerized polypropylene. They are currently the most widely used environmentally friendly shrink films, but they are difficult to recycle due to the use of many different types of polyolefin materials. Polyethylene heat shrink films have high impact strength and high heat sealing strength after processing. Regarding polyethylene shrink films, a Chinese patent document with publication number CN109776926A discloses a PE heat shrink film and a preparation method thereof. The PE heat shrink film provided is prepared from the following raw materials in parts by weight: 50 to 70 parts of low-density polyethylene, 15 to 22 parts of high-density polyethylene, 2 to 5 parts of polyvinyl alcohol, 2 to 5 parts of polyethylene wax, 1 to 4 parts of diatomaceous earth, 1 to 5 parts of calcium carbonate, 2 to 7 parts of kaolin, and 5 to 15 parts of metallocene polyethylene. The preparation of the PE heat shrinkable film prepared by the invention includes the following steps: 1. Prepare relevant raw materials according to the ratio, 2. Send the raw materials to the reaction device for high temperature reaction, 3. Perform mold forming, 4. Punch holes and slitting and rewinding, 5. Pack the finished product. The PE heat shrinkable film prepared by this method has the advantages of good flexibility, strong impact resistance and tear resistance, not easy to break, moisture resistance, high transparency, good strength, and strong toughness. The Chinese patent document with publication number CN109337177A discloses a heat shrinkable film and a preparation method thereof, wherein the heat shrinkable film includes the following components in parts by weight: 100 parts of polyethylene, 1 to 3 parts of antioxidant, 2 to 4 parts of light stabilizer, 0.5 to 1 part of dioctyl terephthalate, 1 to 2 parts of magnesium stearate, 5 to 10 parts of chlorofluorocarbon fiber, and 10 to 15 parts of tussah silk. The heat shrinkable film is obtained by fully stirring and mixing polyethylene, an antioxidant, a light stabilizer, dioctyl terephthalate, magnesium stearate and mixed modified fibers, melting, extruding granulation, blowing film forming and stretching. The heat shrinkable film has strong wear resistance and excellent tensile resistance.The Chinese patent document with publication number CN108177409A discloses a polyethylene heat shrinkable film, which comprises an outermost layer, a second outermost layer, an intermediate layer, a second innermost layer and an innermost layer arranged in sequence, wherein the outermost layer and the innermost layer, the second outermost layer and the second innermost layer are symmetrically distributed with the intermediate layer as the axis, and the thickness ratio of the outermost layer, the second outermost layer, the intermediate layer, the second innermost layer and the innermost layer is (2.5-3.0):(0.5-1.0):(3-6):(0.5-1.0):(2. 5~3.0), in terms of weight percentage, the outermost layer and the innermost layer are composed of 20~40% LDPE, 20~40% HDPE, 20~40% MDPE and 5~20% LLDPE, the sub-outer layer and the sub-inner layer are composed of 10~30% LDPE or LLDPE and 70~90% MLLDPE, and the middle layer is composed of 50~70% HDPE, 20~40% LDPE and 5~15% MDPE. The outermost layer and the innermost layer, the sub-outer layer and the sub-inner layer are all symmetrically distributed with the middle layer as the axis, and the components, contents and thicknesses of each layer of the polyethylene heat shrinkable film are combined to make the polyethylene heat shrinkable film as a whole have high toughness to meet the requirements of high toughness of polyethylene heat shrinkable film in special fields. However, the mechanical properties of the heat shrinkable film disclosed above still need to be improved. Summary of the invention

[0004] In view of this, the present application provides a metallocene polyethylene heat shrinkable film and its composition and preparation method, which overcome the deficiencies of the above-mentioned prior art and can effectively solve the problem that the mechanical properties, heat shrinkage properties and optical properties of the existing polyethylene heat shrinkable film are still difficult to meet the requirements of the packaging field.

[0005] In a first aspect, the present application provides a composition of a metallocene polyethylene heat shrinkable film, the composition comprising composition A, composition B and composition C; wherein,

[0006] The composition A comprises, by weight: 30 to 60 parts of metallocene polyethylene, 20 to 50 parts of octene copolymerized linear metallocene polyethylene, 5 to 30 parts of linear low-density polyethylene and 0 to 5 parts of an additive;

[0007] The B composition comprises, by weight: 30 to 55 parts of metallocene polyethylene, 25 to 40 parts of high-density polyethylene, 10 to 30 parts of linear low-density polyethylene and 0 to 5 parts of an auxiliary agent;

[0008] The C composition comprises, by mass, 30 to 55 parts of metallocene polyethylene, 30 to 55 parts of octene copolymer linear metallocene polyethylene, 5 to 30 parts of linear low-density polyethylene and 0 to 5 parts of additives.

[0009] As an optional embodiment, the auxiliary agent is present in at least one of the composition A, the composition B and the composition C.

[0010] As an optional embodiment, the high-density polyethylene includes a copolymer of ethylene and α-olefin, which has the function of increasing the stiffness of the film in the formulation.

[0011] As an optional embodiment, the density of the high-density polyethylene is 0.940 g / cm 3 Up to 0.960g / cm 3 .

[0012] As an optional embodiment, the melt mass flow rate of the high-density polyethylene is 5.0 g / 10 min to 15.0 g / 10 min.

[0013] As an optional embodiment, the octene copolymer linear metallocene polyethylene includes a copolymer of ethylene and 1-octene, has good mechanical properties and heat sealing properties, and has the function of increasing the film's puncture resistance, heat sealing properties, and sealing properties in the formula.

[0014] As an optional embodiment, the density of the octene copolymer linear metallocene polyethylene is 0.915 g / cm 3 Up to 0.930g / cm 3 .

[0015] As an optional embodiment, the melt mass flow rate of the octene copolymer linear metallocene polyethylene is 0.50 g / 10 min to 1.50 g / 10 min.

[0016] As an optional embodiment, the metallocene polyethylene includes a copolymer of ethylene and α-olefin, has good optical properties and heat-sealing properties, and has the function of improving the heat-sealing properties of the film and improving the optical properties in the formulation.

[0017] As an optional embodiment, the density of the metallocene polyethylene is 0.920 g / cm 3 Up to 0.950g / cm 3 .

[0018] As an optional embodiment, the melt mass flow rate of the metallocene polyethylene is 0.1 g / 10 min to 0.8 g / 10 min.

[0019] In the present invention, α-olefin is used as a comonomer to improve the mechanical properties of polyethylene products.

[0020] As an optional embodiment, the linear low-density polyethylene includes a copolymer of ethylene and α-olefin, has good processing properties, and improves the processing properties in the formulation.

[0021] As an optional embodiment, the density of the linear low-density polyethylene is 0.915 g / cm 3 Up to 0.930g / cm 3 .

[0022] As an optional embodiment, the linear low density polyethylene has a melt mass flow rate of 0.50 g / 10 min to 1.50 g / 10 min.

[0023] As an optional embodiment, when the composition is processed, the composition A, composition B and composition C are respectively added to the silo in proportion as raw materials for the inner layer, middle layer and outer layer, and the film blowing process is carried out through a three-layer co-extrusion blown film equipment to obtain a metallocene polyethylene heat shrinkable film product.

[0024] In the present application, the raw materials of the metallocene polyethylene heat shrinkable film include three compositions, which respectively correspond to the raw materials of the inner layer, the middle layer and the outer layer during processing, and are extruded by a film blowing machine to form the metallocene polyethylene heat shrinkable film product.

[0025] In the present application, the inner, middle and outer layers of the metallocene polyethylene heat shrinkable film have different functions. In addition to maintaining good heat shrinkage performance as a whole, the inner layer is a heat sealing layer with good heat sealing performance and sealing performance, the middle layer is a structural layer, which increases the strength and stiffness of the film, and the outer layer has good printing adaptability, tensile performance and flexibility. In addition, the entire heat shrinkable film has good transparency and glossiness.

[0026] As an optional implementation, the auxiliary agent includes at least one of a processing aid (the main component of which is fluoroelastomer PPA), an open masterbatch, and a color masterbatch.

[0027] In a second aspect, the present application provides a metallocene polyethylene heat shrinkable film, the components of the heat shrinkable film include the composition according to the first aspect of the present invention, the heat shrinkable film includes an inner layer, a middle layer and an outer layer stacked in sequence, wherein the inner layer is a heat sealing layer with good heat sealing performance and sealing performance; the middle layer is a structural layer, which increases the strength and stiffness of the film; the outer layer has good printing adaptability, tensile properties and good flexibility.

[0028] As an optional embodiment, the thickness ratio of the inner layer, the middle layer and the outer layer is 1:(1.1 to 1.5):1.

[0029] The metallocene polyethylene heat shrinkable film of the invention has good heat shrinkage performance, puncture resistance and optical performance.

[0030] As an optional embodiment, the raw material of the inner layer adopts the A composition described in the first aspect of the present invention, that is, the components of the inner layer include, by mass: 30 to 60 parts of metallocene polyethylene, 20 to 50 parts of octene copolymer linear metallocene polyethylene, 5 to 30 parts of linear low density polyethylene and 0 to 5 parts of additives.

[0031] In this layer, metallocene polyethylene ensures the mechanical properties of the film and appropriately reduces the cost, octene copolymer linear metallocene polyethylene provides good mechanical properties and thermal shrinkage properties, and linear low-density polyethylene improves processing performance.

[0032] As an optional embodiment, the raw material of the middle layer adopts the B composition described in the first aspect of the present invention, that is, the components of the middle layer include, by mass: 30 to 55 parts of metallocene polyethylene, 25 to 40 parts of high-density polyethylene, 10 to 30 parts of linear low-density polyethylene and 0 to 5 parts of additives.

[0033] In the present application, the metallocene polyethylene in the middle layer ensures the mechanical properties of the film, the high-density polyethylene improves the stiffness of the film, and the linear low-density polyethylene improves the processing properties.

[0034] As an optional embodiment, the raw material of the outer layer adopts the C composition described in the first aspect of the present invention, that is, the components of the outer layer include, by mass: 30 to 55 parts of metallocene polyethylene, 30 to 55 parts of octene copolymer linear metallocene polyethylene, 5 to 30 parts of linear low density polyethylene and 0 to 5 parts of additives.

[0035] In this layer, metallocene polyethylene ensures the mechanical properties of the film and appropriately reduces the cost, octene copolymer linear metallocene polyethylene provides good mechanical properties and thermal shrinkage properties, and linear low-density polyethylene improves processing performance.

[0036] As an optional embodiment, the auxiliary agent is distributed in at least one of the inner layer, the middle layer and the outer layer.

[0037] As an optional implementation, the thickness of the heat shrinkable film is 0.05 mm to 0.07 mm.

[0038] In a third aspect, the present invention provides a method for preparing the above-mentioned metallocene polyethylene heat shrinkable film, comprising: adding the above-mentioned composition A, composition B and composition C into a silo as raw materials for the inner layer, middle layer and outer layer of the metallocene polyethylene heat shrinkable film, respectively, and performing film blowing processing through a three-layer co-extrusion blown film equipment to obtain the metallocene polyethylene heat shrinkable film.

[0039] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0040] (1) The composition provided in the examples of the present application uses high-density polyethylene, octene copolymerized linear metallocene polyethylene, metallocene polyethylene and linear low-density polyethylene as components, which changes the entanglement effect between polyethylene molecular chains and improves the shrinkage rate of long chain branches in the formula during heat shrinkage. When used to produce heat shrinkable films, the thickness of the product can be reduced and good mechanical properties can be maintained;

[0041] (2) The metallocene polyethylene heat shrinkable film according to the present application is prepared using different raw materials for the inner layer, middle layer and outer layer. The inner layer, middle layer and outer layer in the obtained heat shrinkable film play different roles. In addition to maintaining good heat shrinkage performance as a whole, the inner layer is a heat sealing layer with good heat sealing performance and sealing performance, the middle layer is a structural layer, which increases the strength and stiffness of the film, and the outer layer has good printing adaptability, tensile performance and good flexibility. In addition, the entire heat shrinkable film has good transparency and glossiness. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0043] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0044] Figure 1 It is a schematic diagram of the preparation process of the metallocene polyethylene heat shrinkable film according to the present application. DETAILED DESCRIPTION

[0045] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0046] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0047] According to some embodiments of the first aspect of the present application, a composition of a metallocene polyethylene heat shrinkable film is provided, the composition comprising composition A, composition B and composition C; wherein,

[0048] The composition A comprises, by mass: 30 to 60 parts (e.g., 35, 40, 45, 50 or 55 parts) of metallocene polyethylene, 20 to 50 parts (e.g., 25, 30, 35, 40 or 45 parts) of octene copolymerized linear metallocene polyethylene, 5 to 30 parts (e.g., 10, 15, 20 or 25 parts) of linear low-density polyethylene, and 0 to 5 parts (e.g., 0.5, 1, 2, 3 or 4 parts) of an auxiliary agent;

[0049] The B composition comprises, by mass: 30 to 55 parts (e.g., 35, 40, 45 or 50 parts) of metallocene polyethylene, 25 to 40 parts (e.g., 28, 30, 35 or 38 parts) of high-density polyethylene, 10 to 30 parts (e.g., 12, 15, 20 or 25 parts) of linear low-density polyethylene, and 0 to 5 parts (e.g., 0.5, 1, 2, 3 or 4 parts) of an auxiliary agent;

[0050] The C composition includes, by mass, 30 to 55 parts of metallocene polyethylene, 30 to 55 parts (for example, 35 parts, 40 parts, 45 parts or 50 parts) of octene copolymer linear metallocene polyethylene, 5 to 30 parts (for example, 10 parts, 15 parts, 20 parts or 25 parts) of linear low density polyethylene and 0 to 5 parts (for example, 0.5 parts, 1 parts, 2 parts, 3 parts or 4 parts) of additives.

[0051] In some embodiments, the adjuvant is present in at least one of the A composition, the B composition, and the C composition.

[0052] In this application, the role of high-density polyethylene is to increase the stiffness of the film. If the mass fraction of this component is too large, the adverse effect is to reduce the toughness of the product, and if it is too small, the adverse effect is to reduce the stiffness of the product. High-density polyethylene includes copolymers of ethylene and α-olefins; its density is 0.940g / cm 3 Up to 0.960g / cm 3 ; Its melt mass flow rate is 5.0g / 10min to 15.0g / 10min.

[0053] The function of octene copolymer linear metallocene polyethylene is to increase the mechanical properties of the film and provide good heat shrinkage performance. The disadvantage of taking too large a mass fraction of this component is to increase the production cost, while taking too small a mass fraction is to have insufficient heat shrinkage performance. Octene copolymer linear metallocene polyethylene includes a copolymer of ethylene and 1-octene; its density is 0.915g / cm 3Up to 0.930g / cm 3 ; Its melt mass flow rate is 0.50g / 10min to 1.50g / 10min.

[0054] The role of metallocene polyethylene is to increase the mechanical properties of the film and provide good heat shrinkage performance. The disadvantage of taking too large a mass fraction of this component is that the production cost increases, while the disadvantage of taking too small a mass fraction is that the heat shrinkage performance is insufficient. Metallocene polyethylene includes copolymers of ethylene and α-olefins; its density is 0.920g / cm 3 Up to 0.950g / cm 3 ; Its melt mass flow rate is 0.1g / 10min to 0.8g / 10min.

[0055] The function of linear low-density polyethylene is to improve processing performance. If the mass fraction of this component is too large, the adverse effect is to reduce the mechanical properties of the product. If it is too small, the adverse effect is that the processing performance cannot be effectively improved. Linear low-density polyethylene includes copolymers of ethylene and α-olefins; its density is 0.915g / cm 3 Up to 0.930g / cm 3 ; Its melt mass flow rate is 0.50g / 10min to 1.50g / 10min.

[0056] The composition uses high-density polyethylene, octene copolymer linear metallocene polyethylene, metallocene polyethylene and linear low-density polyethylene as components, changes the entanglement effect between polyethylene molecular chains, and improves the shrinkage rate of long chain branches in the formula during heat shrinkage. When used in the production of heat shrinkable films, the thickness of the product can be reduced and good mechanical properties can be maintained.

[0057] Based on a general inventive concept, some embodiments of the second aspect of the present application further provide a metallocene polyethylene heat shrinkable film, the composition of the heat shrinkable film comprising the composition provided above, the heat shrinkable film comprising an inner layer, a middle layer and an outer layer stacked in sequence; the thickness ratio of the inner layer, the middle layer and the outer layer is 1: (1.1 to 1.5): 1 (for example, 1:1.2:1, 1:1.3:1 or 1:1.4:1).

[0058] In some embodiments, the raw material of the inner layer adopts the A composition described in some embodiments of the first aspect of the present invention, that is, the components of the inner layer include, by mass: 30 to 60 parts of metallocene polyethylene, 20 to 50 parts of octene copolymer linear metallocene polyethylene, 5 to 30 parts of linear low density polyethylene and 0 to 5 parts of additives.

[0059] In some embodiments, the raw material of the middle layer adopts the B composition described in some embodiments of the first aspect of the present invention, that is, the components of the middle layer include, by mass: 30 to 55 parts of metallocene polyethylene, 25 to 40 parts of high-density polyethylene, 10 to 30 parts of linear low-density polyethylene and 0 to 5 parts of additives.

[0060] In some embodiments, the raw material of the outer layer adopts the C composition described in some embodiments of the first aspect of the present invention, that is, the components of the outer layer include, by mass: 30 to 55 parts of metallocene polyethylene, 30 to 55 parts of octene copolymer linear metallocene polyethylene, 5 to 30 parts of linear low density polyethylene and 0 to 5 parts of additives.

[0061] In some embodiments, the heat shrinkable film further comprises an additive, which is distributed in at least one of the inner layer, the middle layer and the outer layer. The additive may be, but is not limited to, a processing aid, an open masterbatch, a color masterbatch, etc. The processing aid may be purchased from the market.

[0062] In some embodiments, the thickness of the heat shrink film is 0.05 mm to 0.07 mm (eg, 0.06 mm).

[0063] According to some embodiments of the third aspect of the present application, a method for preparing a metallocene polyethylene heat shrinkable film is also provided, such as Figure 1 As shown, the preparation method comprises: adding the above-mentioned composition A, composition B and composition C as raw materials for the inner layer, middle layer (or intermediate layer) and outer layer of the metallocene polyethylene heat shrinkable film into a silo, and performing film blowing processing through a three-layer co-extrusion film blowing equipment to obtain the metallocene polyethylene heat shrinkable film.

[0064] In some embodiments, the film blowing process is performed by a three-layer co-extrusion film blowing device, and the thickness of the obtained product is 0.05 mm to 0.07 mm.

[0065] Compared with ordinary heat shrinkable film products, this heat shrinkable film has better mechanical properties, heat shrinkage properties and optical properties, and has more application fields.

[0066] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0067] Example 1

[0068] A heat shrinkable film comprises an inner layer, a middle layer and an outer layer which are stacked in sequence; the thickness ratio of the inner layer, the middle layer and the outer layer is 1:1.3:1.

[0069] The components of the inner layer include, by mass:

[0070] 35 parts of metallocene polyethylene, wherein the metallocene polyethylene is a copolymer of ethylene and 1-hexene;

[0071] 45 parts of octene copolymer linear metallocene polyethylene;

[0072] 17 parts of linear low-density polyethylene, wherein the linear low-density polyethylene is a copolymer of ethylene and 1-butene;

[0073] 3 parts of processing aid (the main component is fluoroelastomer PPA);

[0074] The components of the middle layer include by mass:

[0075] 35 parts of metallocene polyethylene, wherein the metallocene polyethylene is a copolymer of ethylene and 1-hexene;

[0076] 40 parts of high-density polyethylene, wherein the high-density polyethylene is a copolymer of ethylene and 1-hexene;

[0077] 22 parts of linear low-density polyethylene, wherein the linear low-density polyethylene is a copolymer of ethylene and 1-butene;

[0078] 3 parts of processing aid (the main component is fluoroelastomer PPA);

[0079] The components of the outer layer include, by mass:

[0080] 35 parts of metallocene polyethylene, wherein the metallocene polyethylene is a copolymer of ethylene and 1-hexene;

[0081] 40 parts of octene copolymer linear metallocene polyethylene;

[0082] 22 parts of linear low-density polyethylene, wherein the linear low-density polyethylene is a copolymer of ethylene and 1-butene;

[0083] 3 parts of processing aid (the main component is fluoroelastomer PPA).

[0084] The above raw materials are added into the silo according to the formula, and the film is blown through a three-layer co-extrusion film blowing equipment. The thickness of the obtained product is 0.05mm to 0.07mm.

[0085] Example 2

[0086] A heat shrinkable film comprises an inner layer, a middle layer and an outer layer which are stacked in sequence; the thickness ratio of the inner layer, the middle layer and the outer layer is 1:1.3:1.

[0087] The components of the inner layer include, by mass:

[0088] 40 parts of metallocene polyethylene, wherein the metallocene polyethylene is a copolymer of ethylene and 1-hexene;

[0089] 40 parts of octene copolymer linear metallocene polyethylene;

[0090] 17 parts of linear low-density polyethylene, wherein the linear low-density polyethylene is a copolymer of ethylene and 1-butene;

[0091] 3 parts of processing aid (the main component is fluoroelastomer PPA);

[0092] The components of the middle layer include by mass:

[0093] 40 parts of metallocene polyethylene, wherein the metallocene polyethylene is a copolymer of ethylene and 1-hexene;

[0094] 35 parts of high-density polyethylene, wherein the high-density polyethylene is a copolymer of ethylene and 1-hexene;

[0095] 22 parts of linear low-density polyethylene, wherein the linear low-density polyethylene is a copolymer of ethylene and 1-butene;

[0096] 3 parts of processing aid (the main component is fluoroelastomer PPA);

[0097] The components of the outer layer include, by mass:

[0098] 40 parts of metallocene polyethylene, wherein the metallocene polyethylene is a copolymer of ethylene and 1-hexene;

[0099] 35 parts of octene copolymer linear metallocene polyethylene;

[0100] 22 parts of linear low-density polyethylene, wherein the linear low-density polyethylene is a copolymer of ethylene and 1-butene;

[0101] 3 parts of processing aid (the main component is fluoroelastomer PPA).

[0102] The above raw materials are added into the silo in proportion, and the film is blown through a three-layer co-extrusion film blowing equipment. The thickness of the obtained product is 0.05mm to 0.07mm.

[0103] Comparative Example 1

[0104] A heat shrinkable film comprises an inner layer, a middle layer and an outer layer which are stacked in sequence; the thickness ratio of the inner layer, the middle layer and the outer layer is 1:1.2:1.

[0105] The components of the inner layer include, by mass:

[0106] 30 parts of metallocene polyethylene, wherein the metallocene polyethylene is a copolymer of ethylene and 1-hexene;

[0107] 50 parts of low-density polyethylene, wherein the low-density polyethylene is a copolymer of ethylene and 1-butene;

[0108] 17 parts of linear low-density polyethylene, wherein the linear low-density polyethylene is a copolymer of ethylene and 1-butene;

[0109] 3 parts of processing aid (the main component is fluoroelastomer PPA);

[0110] The components of the middle layer include, by mass:

[0111] 30 parts of metallocene polyethylene, wherein the metallocene polyethylene is a copolymer of ethylene and 1-hexene;

[0112] 45 parts of high-density polyethylene, wherein the high-density polyethylene is a copolymer of ethylene and 1-hexene;

[0113] 22 parts of linear low-density polyethylene, wherein the linear low-density polyethylene is a copolymer of ethylene and 1-butene;

[0114] 3 parts of processing aid (the main component is fluoroelastomer PPA);

[0115] The components of the outer layer include by mass:

[0116] 32 parts of metallocene polyethylene, wherein the metallocene polyethylene is a copolymer of ethylene and 1-hexene;

[0117] 45 parts of low-density polyethylene, wherein the low-density polyethylene is a copolymer of ethylene and 1-butene;

[0118] 20 parts of linear low-density polyethylene, wherein the linear low-density polyethylene is a copolymer of ethylene and 1-butene.

[0119] 3 parts of processing aid (the main component is fluoroelastomer PPA).

[0120] The above raw materials are added into the silo in proportion, and the film is blown through a three-layer co-extrusion film blowing equipment. The thickness of the obtained product is 0.05mm to 0.07mm.

[0121] Comparative Example 2

[0122] A heat shrinkable film comprises an inner layer, a middle layer and an outer layer which are stacked in sequence; the thickness ratio of the inner layer, the middle layer and the outer layer is 1:1.4:1.

[0123] The components of the inner layer include, by mass:

[0124] 35 parts of metallocene polyethylene, wherein the metallocene polyethylene is a copolymer of ethylene and 1-hexene;

[0125] 45 parts of low-density polyethylene, wherein the low-density polyethylene is a copolymer of ethylene and 1-butene;

[0126] 17 parts of linear low-density polyethylene, wherein the linear low-density polyethylene is a copolymer of ethylene and 1-butene;

[0127] 3 parts of processing aid (the main component is fluoroelastomer PPA);

[0128] The components of the middle layer include, by mass:

[0129] 35 parts of metallocene polyethylene, wherein the metallocene polyethylene is a copolymer of ethylene and 1-hexene;

[0130] High-density polyethylene 40, wherein the high-density polyethylene is a copolymer of ethylene and 1-hexene;

[0131] 22 parts of linear low-density polyethylene, wherein the linear low-density polyethylene is a copolymer of ethylene and 1-butene;

[0132] 3 parts of processing aid (the main component is fluoroelastomer PPA);

[0133] The components of the outer layer include by mass:

[0134] 35 parts of metallocene polyethylene, wherein the metallocene polyethylene is a copolymer of ethylene and 1-hexene;

[0135] 42 parts of low-density polyethylene, wherein the low-density polyethylene is a copolymer of ethylene and 1-butene;

[0136] 20 parts of linear low-density polyethylene, wherein the linear low-density polyethylene is a copolymer of ethylene and 1-butene.

[0137] 3 parts of processing aid (the main component is fluoroelastomer PPA).

[0138] The above raw materials are added into the silo in proportion, and the film is blown through a three-layer co-extrusion film blowing equipment. The thickness of the obtained product is 0.05mm to 0.07mm.

[0139] The compositions provided in the above embodiments and comparative examples were blown into films in a film blowing machine, and the product films were subjected to performance tests, including: film tensile properties: tested in accordance with GB / T 1040.3, dumbbell-shaped specimens, and a stretching speed of 200 mm / min.

[0140] Dart impact damage quality: tested in accordance with GB / T 9639.1.

[0141] Film right-angle tear strength: tested in accordance with QB / T 1130.

[0142] Film haze / transmittance: tested in accordance with GB / T 2410.

[0143] The test results are shown in Table 1 below.

[0144] Table 1:

[0145]

[0146] It can be seen from the data in Table 1 above that the heat shrinkable film made using the composition provided in the examples of the present application has better mechanical properties and optical properties.

[0147] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0148] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the present specification, the terms "including", "comprising", etc. refer to "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of the associated objects, indicating that there may be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plural" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items (individuals) or plural items (individuals). For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc, or abc, where a, b, c can be single or plural, respectively.

[0149] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A composition of a metallocene polyethylene heat shrinkable film, characterized in that: The composition includes composition A, composition B and composition C; wherein, The composition A comprises, by weight: 35 to 40 parts of metallocene polyethylene, 40 to 45 parts of octene copolymerized linear metallocene polyethylene, 17 parts of linear low-density polyethylene and 3 parts of an additive, wherein the metallocene polyethylene is a copolymer of ethylene and 1-hexene; The B composition comprises, by weight: 35 to 40 parts of metallocene polyethylene, 35 to 40 parts of high-density polyethylene, 22 parts of linear low-density polyethylene and 3 parts of an additive, wherein the metallocene polyethylene is a copolymer of ethylene and 1-hexene; The C composition comprises, by weight: 35 to 40 parts of metallocene polyethylene, 35 to 40 parts of octene copolymerized linear metallocene polyethylene, 22 parts of linear low-density polyethylene and 3 parts of an additive, wherein the metallocene polyethylene is a copolymer of ethylene and 1-hexene; The octene copolymer linear metallocene polyethylene comprises a copolymer of ethylene and 1-octene; the density of the octene copolymer linear metallocene polyethylene is 0.915 g / cm 3 Up to 0.930g / cm 3 ; The melt mass flow rate of the octene copolymer linear metallocene polyethylene is 0.50 g / 10 min to 1.50 g / 10 min; The A composition is used as an inner layer, the B composition is used as a middle layer, and the C composition is used as an outer layer. The inner layer, the middle layer, and the outer layer are stacked in sequence to obtain a heat shrinkable film. The thickness ratio of the inner layer, the middle layer, and the outer layer is 1:(1.1-1.5):1, and the thickness of the heat shrinkable film is 0.05-0.07 mm; The density of the high-density polyethylene is 0.940 g / cm 3 Up to 0.960g / cm 3 ; The melt mass flow rate of the high-density polyethylene is 5.0 g / 10 min to 15.0 g / 10 min; The density of the metallocene polyethylene is 0.920 g / cm 3 Up to 0.950g / cm 3 ; The melt mass flow rate of the metallocene polyethylene is 0.1 g / 10 min to 0.8 g / 10 min; The density of the linear low-density polyethylene is 0.915 g / cm 3 Up to 0.930g / cm 3 ; The melt mass flow rate of the linear low density polyethylene is 0.50g / 10min to 1.50g / 10min.

2. A method for preparing a metallocene polyethylene heat shrinkable film according to claim 1, characterized in that: The preparation method comprises the following steps: adding the composition A, the composition B and the composition C as claimed in claim 1 into a silo as raw materials for the inner layer, the middle layer and the outer layer of the metallocene polyethylene heat shrinkable film respectively, and performing film blowing processing through a three-layer co-extrusion film blowing equipment to obtain the metallocene polyethylene heat shrinkable film.

Citation Information

Patent Citations

  • Polyethylene thermal shrinkage film

    CN108177409A

  • Heat-shrinkable film and preparation method thereof

    CN109337177A

  • PE thermal shrinkage film and preparation method thereof

    CN109776926A

  • Low-temperature-resistant three-layer co-extrusion heavy packaging film

    CN115635750A