A method for preparing an adhesive for aluminum-wood composite

By using an adhesive with a phosphorus, chromium, magnesium component and a modified polymer component between aluminum alloy and wood-plastic materials, the bonding force problem caused by the difference in polarity of the materials is solved, and an adhesive effect of high strength and water resistance is achieved. , to avoid hydrolysis and degradation and blackening.

CN117567981BActive Publication Date: 2024-10-15HUANGSHAN BANNER TECH
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202311366121.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-20
Publication Date
2024-10-15
Estimated Expiration
2043-10-20

AI Technical Summary

Technical Problem

The difference in polarity between aluminum alloy and wood-plastic fabrics results in direct bonding without bonding force. Adhesives are required for bonding, but existing adhesives cannot effectively solve this problem.

Method used

An adhesive preparation method using phosphorus, chromium and magnesium components and modified polymer components is used to form a high-strength grafted polymer through the dehydration condensation of phosphoric acid, chromium oxide, and magnesium borate and the condensation reaction of polyvinyl alcohol and formaldehyde. , and form a phosphorus ester bond through the esterification reaction of carboxyl groups and polyamide to improve the bonding performance.

Benefits of technology

A high-strength and water-resistant adhesive is achieved that can effectively bond aluminum alloys and wood-plastic materials, avoid hydrolysis and degradation and blackening, and exhibit good tensile strength and peel strength.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of adhesives, and in particular to a method for preparing an adhesive for aluminum-wood composites, comprising a phosphorus-chromium-magnesium component and a modified polymer component; the method for preparing the phosphorus-chromium-magnesium component is as follows: adding deionized water, phosphoric acid, and chromium oxide in proportion to a container, stirring and reacting at 80-90° C. until the solution is clear, continuing to add magnesium borate, and after the reaction is completed, adding deionized water to adjust the density to 1.4-1.6 g / cm 3 , cooling and discharging; the preparation method of the modified polymer component is as follows: add deionized water and polyvinyl alcohol in proportion to a container, heat and stir until the polyvinyl alcohol is completely dissolved, cool to 30-40°C, add 37% formaldehyde solution to react, add acid to adjust the pH to 1-3, heat to 80-90°C, add polyamide containing carboxyl, and after the reaction is completed, cool and discharge. The composite adhesive prepared by the present invention has excellent performance, with a tensile strength of 25.3Mpa, an elongation at break of 658%, and a peel strength of 275N / 25mm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adhesives, and in particular to a method for preparing an adhesive for aluminum-wood composites. Background Art

[0002] Aluminum-wood composite material is an emerging wood-plastic product. As a green product, it is made of biodegradable wood-plastic sheet and recyclable aluminum alloy through co-extrusion. The wood-plastic layer is used as the decorative layer, and the aluminum alloy is used as the load-bearing layer. The product is beautiful and atmospheric. As a courtyard building material, it is light in weight, high in strength, and low in price. It can replace ordinary metal and concrete structures. Its products are generally made by co-extruding and coating the adhesive resin on the surface of the aluminum alloy and then co-extruding the wood-plastic sheet for thermal compounding. Due to the difference in polarity between the wood-plastic fabric and the aluminum alloy, there is no bonding force when directly combined. Therefore, it is necessary to use adhesives to bond the aluminum alloy surface and the wood-plastic fabric. Summary of the invention

[0003] In order to solve the problems mentioned in the above background technology, the present invention provides a method for preparing an adhesive for aluminum-wood composite.

[0004] In order to achieve the above object, the present invention adopts the following technical solutions:

[0005] A method for preparing an adhesive for aluminum-wood composite, comprising a phosphorus-chromium-magnesium component and a modified polymer component;

[0006] The preparation method of the phosphorus-chromium-magnesium component is as follows:

[0007] Add deionized water, phosphoric acid, and chromium oxide in proportion to the container, stir and react at 80-90°C until the solution is clear, continue to add magnesium borate, and after the reaction is completed, add deionized water to adjust the density to 1.4-1.6g / cm 3 , cooling and discharging;

[0008] The preparation method of the modified polymer component is as follows:

[0009] Add deionized water and polyvinyl alcohol in proportion to a container, heat and stir until the polyvinyl alcohol is completely dissolved, cool to 30-40°C, add 37% formaldehyde solution to react, add acid to adjust the pH to 1-3, heat to 80-90°C, add polyamide containing carboxyl groups, and after the reaction is completed, cool and discharge.

[0010] Preferably, the preparation method of the polyamide containing carboxyl groups is as follows:

[0011] Under a nitrogen atmosphere, add DMF, 1,3,5-cyclohexanetricarboxylic acid, hexamethylenediamine and pyridine in proportion to a container, stir until all are dissolved, add triphenyl phosphite, react at 20-30°C for 1-2h, 60-80°C for 1-2h, and 100-120°C for 1-2h. After the reaction, add deionized water, precipitate, filter, wash and dry, re-precipitate with acetone and dry to obtain a polyamide containing a carboxyl group.

[0012] Preferably, the mass volume ratio of the deionized water, phosphoric acid, chromium oxide and magnesium borate is: 100 ml: (100-120 g): (30-50 g): (80-120 g).

[0013] Preferably, the mass volume ratio of the deionized water, polyvinyl alcohol, 37% formaldehyde solution, and polyamide containing carboxyl group is 100 ml: (10-20 g): (5-10 g): (10-20 g).

[0014] Preferably, the mass volume ratio of DMF, 1,3,5-benzenetricarboxylic acid, hexamethylenediamine, pyridine and triphenyl phosphite is 100 ml: (20-30 g): (10-15 g): (5-10 g): (5-10 g).

[0015] Preferably, the mass ratio of the phosphorus-chromium-magnesium component to the modified polymer component is 1:(0.5-2).

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] 1. The synthesized adhesive for aluminum-wood composites of the present invention comprises a phosphorus-chromium-magnesium component and a modified polymer component. Phosphoric acid, chromium oxide, and magnesium borate are dehydrated and condensed to form polychromic magnesium phosphate. The condensation reaction of polyvinyl alcohol and formaldehyde is step-by-step, first forming hemiacetal, then forming carbon cations, and finally generating acetal. Under acidic heating conditions, the hydroxyl groups in the polyvinyl alcohol formal molecule react with the carboxyl groups in the polyamide molecule containing carboxyl groups to form a grafted polymer with a carbon-oxygen ring and a benzene ring structure. This polymer exhibits high strength and water resistance, and can react with the phosphorus hydroxyl groups in the polychromic magnesium phosphate through the carboxyl groups to form a phosphoester bond.

[0018] 2. The synthesized adhesive for aluminum-wood composites of the present invention comprises a phosphorus-chromium-magnesium component and a modified polymer component. The phosphorus-chromium-magnesium component is an inorganic adhesive and has good bonding properties to wood-plastics. The modified polymer component contains carboxyl and amide groups, has good affinity to many materials, has good intermolecular forces, and has good bonding ability to metals in particular. The carboxyl in the modified polymer component undergoes an esterification reaction with the phosphorus hydroxyl in the chromium-magnesium polyphosphate to form a phosphoester bond, which can avoid the phosphate radical from contacting with the water molecules in the wood-plastics and hydrolyzing them, and avoids the degradation and blackening of the wood-plastics in the bonding layer. The adhesive firmly grasps the wood through a small amount of hydrogen bonds and penetrates into the gaps of the bonding surfaces to form "glue nails" to exert an adhesive effect.

[0019] 3. The composite adhesive prepared by the present invention has excellent performance, with a tensile strength of 25.3Mpa, an elongation at break of 658%, and a peel strength of 275N / 25mm. DETAILED DESCRIPTION

[0020] Unless otherwise specified, the parts in the present invention are parts by mass;

[0021] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.

[0022] Among them, polyvinyl alcohol was purchased from Aladdin, with a degree of alcoholysis of 87.0-89.0% (mol / mol).

[0023] Preparation Example 1

[0024] The preparation method of polyamide containing carboxyl group is as follows:

[0025] Under a nitrogen atmosphere, DMF, 1,3,5-cyclohexanetriolic acid, hexamethylenediamine and pyridine were added in proportion to a container, stirred until completely dissolved, triphenyl phosphite was added, and the reaction was carried out at 25°C for 1.5 h, 70°C for 1.5 h, and 110°C for 1.5 h. After the reaction, deionized water was added, the mixture was precipitated, filtered, washed, and dried. The mixture was re-precipitated with acetone and dried to obtain a polyamide containing a carboxyl group.

[0026] The mass volume ratio of the DMF, 1,3,5-benzenetricarboxylic acid, hexamethylenediamine, pyridine and triphenyl phosphite is 100 ml: 25 g: 12.5 g: 7.5 g: 7.5 g.

[0027] Preparation Example 2

[0028] The difference between this preparation example and preparation example 1 is that the mass volume ratio of DMF, 1,3,5-benzenetricarboxylic acid, hexamethylenediamine, pyridine and triphenyl phosphite is 100ml:20g:10g:5g:5g, and the rest is exactly the same as preparation example 1.

[0029] Preparation Example 3

[0030] The difference between this preparation example and preparation example 1 is that the mass volume ratio of DMF, 1,3,5-benzenetricarboxylic acid, hexamethylenediamine, pyridine and triphenyl phosphite is 100ml:30g:15g:10g:10g, and the rest is exactly the same as preparation example 1. Example 1

[0031] A method for preparing an adhesive for aluminum-wood composite, comprising a phosphorus-chromium-magnesium component and a modified polymer component; the mass ratio of the phosphorus-chromium-magnesium component to the modified polymer component is 1:1;

[0032] The preparation method of the phosphorus-chromium-magnesium component is as follows:

[0033] Add deionized water, phosphoric acid, and chromium oxide in proportion to the container, stir and react at 85°C until the solution becomes clear, continue to add magnesium borate, and after the reaction is complete, add deionized water to adjust the density to 1.5 g / cm 3 , cooling and discharging;

[0034] The mass volume ratio of the deionized water, phosphoric acid, chromium oxide and magnesium borate is: 100ml: 110g: 40g: 100g;

[0035] The preparation method of the modified polymer component is as follows:

[0036] Add deionized water and polyvinyl alcohol in proportion to a container, heat and stir until the polyvinyl alcohol is completely dissolved, cool to 35°C, add 37% formaldehyde solution (mass fraction) to react, add acid to adjust the pH to 2, heat to 85°C, add carboxyl-containing polyamide (obtained in Preparation Example 1), and after the reaction is completed, cool and discharge.

[0037] The mass volume ratio of the deionized water, polyvinyl alcohol, 37% formaldehyde solution, and the polyamide containing carboxyl groups (obtained in Preparation Example 1) is 100 ml: 15 g: 7.5 g: 15 g. Example 2

[0038] The difference between this embodiment and embodiment 1 is that the mass ratio of the phosphorus-chromium-magnesium component to the modified polymer component is 1:0.5, and the rest is exactly the same as embodiment 1. Example 3

[0039] The difference between this embodiment and embodiment 1 is that the mass ratio of the phosphorus-chromium-magnesium component to the modified polymer component is 1:2, and the rest is exactly the same as embodiment 1. Example 4

[0040] The difference between this embodiment and embodiment 1 is that the mass volume ratio of the deionized water, phosphoric acid, chromium oxide and magnesium borate is 100 ml: 100 g: 30 g: 80 g, and the rest is exactly the same as embodiment 1. Example 5

[0041] The difference between this embodiment and embodiment 1 is that the mass volume ratio of the deionized water, phosphoric acid, chromium oxide and magnesium borate is 100 ml: 120 g: 50 g: 120 g, and the rest is exactly the same as embodiment 1. Example 6

[0042] The difference between this embodiment and embodiment 1 is that the mass volume ratio of the deionized water, polyvinyl alcohol, 37% formaldehyde solution, and polyamide containing carboxyl group is 100ml:10g:5g:10g, and the rest is exactly the same as embodiment 1. Example 7

[0043] The difference between this embodiment and embodiment 1 is that the mass volume ratio of the deionized water, polyvinyl alcohol, 37% formaldehyde solution, and polyamide containing carboxyl group is 100ml:20g:10g:20g, and the rest is exactly the same as embodiment 1.

[0044] Results and Testing

[0045] 1. Mechanical properties test

[0046] When testing the tensile strength, the phosphorus-chromium-magnesium component and the modified polymer component were first mixed uniformly in proportion, dried in an oven at 120° C. for 6 h, and prepared into test samples according to ASTM D638 standard. The tensile strength and elongation at break of the samples prepared according to Examples 1-7 were tested using an AGS-X500N universal testing machine, and the tensile rate during the test was 50 mm / min. The results are shown in Table 1.

[0047] Table 1

[0048] Tensile strength (Mpa) Elongation at break % Example 1 25.3 658 Example 2 23.1 635 Example 3 22.8 612 Example 4 22.7 605 Example 5 22.1 621 Example 6 23.4 619 Example 7 23.8 637

[0049] 2. Peel strength test

[0050] The test films of Examples 1-7 were made into 0.1 mm thick, 25 mm wide and 50 mm long films by hot pressing with a mold. The films were placed between an aluminum sheet and a wood-plastic board, and hot pressed into three-layer composite sheets at 120° C. and 0.3 MPa pressure. The peel strength at 90° C. was tested according to the international standard ISO 8510-2-2006, and the tensile speed was 50 mm / min. The results are shown in Table 2.

[0051] Table 2

[0052] Peel strength (N / 25mm) Example 1 275 Example 2 253 Example 3 254 Example 4 249 Example 5 259 Example 6 248 Example 7 251

[0053] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing an adhesive for aluminum-wood composite, characterized in that: It comprises a phosphorus-chromium-magnesium component and a modified polymer component; the mass ratio of the phosphorus-chromium-magnesium component to the modified polymer component is 1:1; The preparation method of the phosphorus-chromium-magnesium component is as follows: Add deionized water, phosphoric acid, and chromium oxide in proportion to the container, stir and react at 85°C until the solution becomes clear, continue to add magnesium borate, and after the reaction is complete, add deionized water to adjust the density to 1.5 g / cm 3 , cooling and discharging; The mass volume ratio of the deionized water, phosphoric acid, chromium oxide and magnesium borate is 100ml:110g:40g:100g; The preparation method of the modified polymer component is as follows: Add deionized water and polyvinyl alcohol in proportion to a container, heat and stir until the polyvinyl alcohol is completely dissolved, cool to 35°C, add 37% formaldehyde solution by mass to react, add acid to adjust the pH to 2, heat to 85°C, add polyamide containing carboxyl groups, and after the reaction is completed, cool and discharge; The mass volume ratio of the deionized water, polyvinyl alcohol, 37% formaldehyde solution, and carboxyl-containing polyamide is 100 ml: 15 g: 7.5 g: 15 g; The preparation method of polyamide containing carboxyl group is as follows: Under a nitrogen atmosphere, DMF, 1,3,5-benzenetricarboxylic acid, hexamethylenediamine, and pyridine were added in proportion to a container, stirred until all dissolved, triphenyl phosphite was added, reacted at 25°C for 1.5 h, 70°C for 1.5 h, and 110°C for 1.5 h. After the reaction, deionized water was added, precipitated, filtered, washed, dried, reprecipitated with acetone, and dried to obtain a polyamide containing a carboxyl group; The mass volume ratio of the DMF, 1,3,5-benzenetricarboxylic acid, hexamethylenediamine, pyridine and triphenyl phosphite is 100 ml: 25 g: 12.5 g: 7.5 g: 7.5 g.

Citation Information

Patent Citations

  • Aluminum wood composite veneer and processing method thereof

    CN101811314A

  • Method for manufacturing aluminum plastic-wooden composite buckle

    CN102817454A

  • Ultra-low temperature composite hot melt adhesive membrane for aluminum board and fireproof board and preparation method of composite hot melt adhesive membrane

    CN103173146A

  • Primer for metal substrate structural bonding and preparation method thereof

    CN103242792A

  • High-toughness polyvinyl butyral film and preparation method thereof

    CN104910822A