A super lubricating graphene intercalation CN x Thin film construction method

Depositing graphene intercalated CNx film in mechanical systems through high-power pulse magnetron sputtering technology solves the problem of friction and wear in mechanical systems, and achieves superlubrication effect in various environments, reducing friction coefficient and improving Material wear resistance and reliability.

CN117587375BActive Publication Date: 2024-11-15LANZHOU INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311687307.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-11
Publication Date
2024-11-15
Estimated Expiration
2043-12-11

AI Technical Summary

Technical Problem

Friction and wear in mechanical systems lead to high energy consumption and component failure. The existing technology is difficult to effectively reduce friction and wear, limiting the high accuracy, high reliability and long-life operation of the mechanical system.

Method used

High-power pulsed unequilibrium magnetron sputtering technology is used to deposit graphene intercalated CNx film on the substrate surface, and the graphite central column target and nitrogen as carbon and nitrogen sources are used to prepare a super-lubricated nitrogen-doped diamond amorphous carbon coating. , form a cauliflower-like structure to improve lubricating performance.

Benefits of technology

It achieves a low friction coefficient under a variety of environments (including inert gas and current-carrying conditions), achieving a superlubricated state, reducing friction and wear, improving material wear resistance and reliability, and reducing energy losses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117587375B_ABST
    Figure CN117587375B_ABST
Patent Text Reader

Abstract

The invention discloses a super lubricating graphene intercalation CN x The film construction method is to use a graphite central column target as a carbon source and nitrogen as a nitrogen source, and use high-power pulsed unbalanced magnetron sputtering technology to prepare a graphene intercalation CN on the substrate surface. x The prepared CN x In the film, the nitrogen doping amount is not less than 10.0 wt%, the carbon content is not less than 87.81 wt%, sp 3 The carbon content of the structure is at least 82 at%, and it has a graphene intercalation structure. x The film exhibits an ultra-low friction coefficient in an inert gas environment, and can reach a superlubricity state (μ < 0.01) when sliding with a variety of pairs in atmospheres such as nitrogen and argon, showing good friction and wear properties, achieving superlubricity on a macro scale.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for constructing a superlubricating CNx film, in particular to a method for constructing a superlubricating graphene intercalation CNx film, and belongs to the field of engineering materials and the field of tribological lubrication technology. Background Art

[0002] About 1 / 3 of the world's primary energy is consumed by friction in mechanical systems. On the other hand, 60% of machine parts failures are caused by wear. The high precision, high reliability and long service life of mechanical systems are limited by the friction and wear properties of materials. Reliable means and technologies to reduce friction and wear are the key to achieving low energy consumption, high reliability and long life operation of mechanical systems. Superlubrication refers to a state where the friction coefficient is less than 0.01 and the friction coefficient approaches zero (0.001 or less); compared with conventional lubrication, the friction coefficient and wear rate are reduced by orders of magnitude. Superlubrication was first proposed in 1990. After the stages of structural superlubrication, two-dimensional material superlubrication, homogeneous and heterogeneous superlubrication, and thin film superlubrication, superlubrication technology has been greatly developed and applied. The emergence of ultra-low friction and superlubrication technology provides a new option for solving the above-mentioned engineering problems, which is expected to solve a series of problems such as friction, wear, and energy of components from the root, and bring about comprehensive technological innovation.

[0003] Carbon-based materials have excellent friction properties. In the field of tribology, especially in the research of solid superlubrication, carbon-based materials account for more than 95%. Among them, amorphous carbon coatings can be deposited on the surface of metal substrates and have high load-bearing capacity. It is one of the most promising coatings for achieving engineering superlubrication and application. The excellent tribological properties and high wear resistance of amorphous carbon nitride film (CNx) in an inert gas environment have attracted the interest of many researchers in the past. As a kind of sp 2 CN and sp 3 The hybrid material composed of CN bonding has ultra-low friction in a dry inert gas environment, especially in nitrogen. Some people believe that the mechanism of ultra-low friction is that nitrogen atoms desorb from the surface of the CNx coating during the running-in period, and the friction surface becomes a carbon-rich friction layer similar to graphite, and an extremely thin transfer layer is formed on the surface of the dual ball. There are also views such as "nitrogen lubrication". In view of this, the study of low friction surfaces of CNx films is particularly important. Summary of the invention

[0004] In view of the above technical problems, the present invention provides a super lubricating graphene intercalation structure CN x A method for constructing a friction pair is provided to improve the lubrication performance of the diamond-like carbon coating material and avoid excessive friction and wear of the workpiece and unnecessary energy loss.

[0005] The present invention is a super lubricating graphene intercalation CN xThe film construction method is to use a graphite central column target as a carbon source and nitrogen as a nitrogen source, and use high-power pulsed unbalanced magnetron sputtering technology to prepare a graphene intercalation CN on the substrate surface. x Film. It specifically includes the following process steps:

[0006] (1) Cleaning of substrate: The substrate was ultrasonically cleaned with petroleum ether, anhydrous ethanol, and deionized water respectively. After drying, it was placed on the rotating rack of the vacuum coating chamber of the magnetron sputtering device. The target distance between the substrate and the graphite center column target was adjusted to 11-15 cm, and the vacuum was evacuated to 5×10 -3 Pa, turn on the rotating rack and rotate the graphite center column target, and the graphite target and the rack rotate at a constant speed in the opposite direction.

[0007] The substrate is an oriented (10 0) single crystal silicon wafer, and the graphite center column target is a 4000 magnetic flux samarium cobalt magnet (Sm2Co 17 ).

[0008] (2) Preparation of nitrogen-doped diamond-like amorphous carbon film: Argon and nitrogen are introduced, and the working pressure of the chamber is adjusted to 0.54~0.68 Pa; at the same time, the power supply of the high-power pulse is adjusted to deposit the graphene intercalation structure CN on the substrate surface. x film:

[0009] The flow rate of argon gas was controlled at 160sccm, the flow rate of nitrogen gas was switched from 50sccm to 20sccm every 6 minutes, the high-power pulse power supply was changed synchronously with 1200V, 650V and nitrogen gas (1200V corresponds to 50sccm, 650V corresponds to 20sccm), the current of graphite target was 100A, the output power was changed synchronously with 12kW, 6.5KW and nitrogen gas (12kW corresponds to 50sccm, 6.5KW corresponds to 20sccm), and the bias voltage was 70V. The cycle was repeated until the thickness of diamond-like amorphous carbon coating reached the target thickness.

[0010] During the whole process, the rotation speed of the graphite target and the workpiece is 0.114 m / s, and the pulse power supply and gas supply are synchronized. Figure 1 .

[0011] Figure 2 The graphene intercalation structure CN prepared by the present invention x The surface (a) and cross-sectional SEM images (b) of the film show that after high-power magnetron sputtering deposition, a large number of cauliflower-like structures are formed on the surface of the silicon wafer, while the side of the coating grows in a columnar manner.

[0012] Figure 3 The nitrogen-doped diamond-like amorphous carbon CN prepared by the present invention xThe 5 × 5 μm AFM image of the film shows that the coating roughness is close to 4.80 nm as measured by AFM, and the smoothness is extremely high. High-power magnetron sputtering has high ionization and high energy, which can deposit smooth and dense films, which is beneficial to tribological properties.

[0013] Figure 4 The nitrogen-doped diamond-like amorphous carbon CN prepared by the present invention x The friction coefficient diagram of the film in a nitrogen atmosphere under a load of 1N and paired with a 440C steel ball to achieve superlubricity for 43min (8666 revolutions). After about 330s of pre-running in a 50% humid atmosphere, the CNx film achieved superlubricity for 43min in a nitrogen atmosphere with humidity < 3%, entering the superlubricity state quickly and lasting for a long time.

[0014] Figure 5 This is a high-resolution HRTEM image of the CNx film surface after the friction test. It can be seen that a polymer-like surface microstructure and a clear graphene strip structure are generated after friction. It is speculated that this polymer-like composite graphene tissue microstructure is the reason why the CNx film quickly enters the superlubrication state in an inert gas environment.

[0015] through Figure 6 XPS photoelectron spectroscopy analysis shows that the nitrogen doping amount of the prepared nitrogen-doped diamond-like amorphous carbon coating is not less than 10.0 wt%, the carbon content is not less than 87.81 wt%, and the surface oxidation is very little.

[0016] After testing, the nitrogen-doped diamond-like amorphous carbon CN prepared by the present invention x The film exhibits an ultra-low friction coefficient in an inert gas environment, especially in nitrogen and argon atmospheres. A variety of pairs can reach a super-lubricating state (440C steel balls, alumina ceramic balls, silicon nitride ceramic balls), showing good friction and wear properties. The friction coefficient is less than 0.01, and the lowest can reach 0.003, achieving super-lubricating performance on a macro scale.

[0017] The surface polymer composite graphene structure is pre-grown in a hydrogen peroxide (humidity 15-90%) atmosphere. This structure is considered to be the origin of the superlubricity of the CNx film. Then, in an atmosphere of nitrogen, argon, etc., or under current conditions, sliding with a variety of pairs (440C steel balls, alumina and silicon nitride ceramic balls) can achieve superlubricity.

[0018] In summary, the present invention has the following advantages over the prior art:

[0019] 1. The present invention achieves superlubricity under various inert gases and even current-carrying conductive environments by pre-running and growing graphene intercalated CNx films, and is expected to realize the engineering application of superlubricity technology under cross-environmental conditions;

[0020] 2. The present invention is used to prepare graphene intercalation CN x During the film formation process, synchronous pulse power supply and gas supply are used to achieve orderly control of graphene intercalation, ensuring high doping content and CN x The quality of the membrane structure;

[0021] 3. The preparation process of the present invention does not involve high temperature process, which effectively avoids grain growth and unnecessary energy loss, reduces preparation cost, and is conducive to promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The nitrogen-doped diamond-like amorphous carbon CN prepared by the present invention x Schematic diagram of the pulsed gas and power supply to the membrane.

[0023] Figure 2 The nitrogen-doped diamond-like amorphous carbon CN prepared by the present invention x Surface and cross-sectional SEM images of the films.

[0024] Figure 3 The nitrogen-doped diamond-like amorphous carbon CN prepared by the present invention x 5 × 5 μm AFM image of the film.

[0025] Figure 4 The nitrogen-doped diamond-like amorphous carbon CN prepared by the present invention x Friction coefficient diagram of the film in nitrogen atmosphere under 1N load paired with 440C steel ball to achieve superlubrication for 43min (8666 revolutions).

[0026] Figure 5 This is a high-resolution electron microscope photograph of the nitrogen-doped diamond-like amorphous carbon CNx film prepared in the present invention.

[0027] Figure 6 This is the full XPS spectrum of the nitrogen-doped diamond-like amorphous carbon CNx film prepared in the present invention.

[0028] Figure 7 The nitrogen-doped diamond-like amorphous carbon CN prepared by the present invention x Friction coefficient diagram of the film in nitrogen atmosphere with different pairings under 1N load.

[0029] Figure 8 The nitrogen-doped diamond-like amorphous carbon CN prepared by the present invention x Friction coefficient diagram of the film paired with a 440C steel ball in different atmospheres under a load of 1N.

[0030] Fig. 9 The nitrogen-doped diamond-like amorphous carbon CN prepared by the present invention xComparison of the superlubricating friction coefficient of the film under no current and current conditions. DETAILED DESCRIPTION

[0031] The nitrogen-doped diamond-like amorphous carbon CN of the present invention is described in detail below through specific examples. x The preparation method of the film and its friction properties are described in detail.

[0032] (1) Cleaning of substrate: The oriented (10 0) single crystal silicon wafer substrate was ultrasonically cleaned with petroleum ether, alcohol and deionized water for 10 min respectively, and then baked in a vacuum oven at 110°C for 120 min to remove the moisture and some volatile organic matter adsorbed on the surface of the material;

[0033] (2) Nitrogen-doped diamond-like amorphous carbon (CN) x Preparation of thin films: Place the cleaned silicon wafer in the rotating rack of the vacuum chamber in the magnetron sputtering device, adjust the distance between the graphite center column target and the workpiece (silicon wafer) to 15 cm, and evacuate to 5×10 -3 Pa, turn on the rotating device, and make the graphite target and the workbench rotate at a constant speed in the opposite direction (the speed is 0.114 m / s). Argon and nitrogen are introduced, and the working pressure of the chamber is adjusted to 0.68 Pa. The nitrogen-doped diamond-like amorphous carbon coating is deposited by unbalanced magnetron sputtering technology. Among them, the argon flow rate is maintained at 160 sccm, and the nitrogen flow rate is switched from 500 sccm to 20 sccm every 6 minutes; the current of the graphite target is 100A, the output power is 1200, 650 W, and it is switched synchronously with nitrogen every 6 minutes; the bias voltage is -70V, the deposition time is 60 min, and the nitrogen-doped diamond-like amorphous carbon CN x The thickness of the film is 860nm;

[0034] (3) Testing of friction performance of different pairs: Using CSM, 440C steel balls, Al2O3, Si3N4, ZrO2, SiC ceramic balls, and glass balls were used as friction pairs. They were pre-runned for 330 seconds under a load of 1N and in various atmospheres with a humidity of 15% using hydrogen peroxide. The friction coefficients were then measured in a nitrogen environment with a humidity of <3%. The results are shown in Table 1. Figure 7 It can be seen that the prepared samples can achieve superlubricity when sliding with various pairs (440C steel balls, alumina and silicon nitride ceramic balls) in a nitrogen atmosphere.

[0035] Table 1 Friction properties of different pairs of prepared samples

[0036]

[0037] (4) Testing of friction performance in different atmospheres: Using CSM, with steel balls as the friction pair, pre-running for 330 s in various atmospheres (nitrogen, argon, oxygen, helium, vacuum) with a load of 1N and humidity controlled by hydrogen peroxide at 90%, and then measuring the friction coefficient in different atmospheres with humidity less than 3%. The results are shown in Table 2. Figure 8 It can be seen that the prepared samples exhibit good friction and wear properties in nitrogen, argon and other atmospheres, and can reach a superlubricity state.

[0038] Table 2 Friction properties of samples prepared in different atmospheres

[0039]

[0040] (5) Test of friction performance under DC supply current: Using CSM friction machine, with steel balls as friction pairs, pre-running for 330 seconds in an atmospheric environment with a load of 1N and a humidity of 50%. Then, in a nitrogen atmosphere with a humidity of less than 3%, the supply DC current was changed from 0.15 to 1.5A, and the friction coefficient was measured. The results are as follows: Fig. 9 The Carrier-free curve is the friction coefficient curve of the CNx film prepared at high power without current, and the Effective-current curve is the friction curve of the same film with direct current, and the friction coefficient of the current-carrying curve is about 0.006.

Claims

1. A super-lubricating graphene intercalation CN x The film construction method is to use a graphite central column target as a carbon source and nitrogen as a nitrogen source, and use high-power pulsed unbalanced magnetron sputtering technology to prepare a graphene intercalation CN on the substrate surface. x Film; which specifically includes the following process steps: (1) Cleaning of substrate: The substrate was ultrasonically cleaned with petroleum ether, anhydrous ethanol, and deionized water respectively. After drying, it was placed on the rotating rack of the vacuum coating chamber of the magnetron sputtering device. The distance between the substrate and the graphite center column target was adjusted and the vacuum was evacuated to 5 × 10 - 3 Pa, turn on the rotating frame and rotate the graphite center column target, and the graphite target and the frame rotate at a constant speed in the opposite direction; (2) Preparation of nitrogen-doped diamond-like amorphous carbon film: Argon and nitrogen are introduced, and the working pressure of the chamber is adjusted to 0.54~0.68 Pa; at the same time, the power supply of the high-power pulse is adjusted to deposit the graphene intercalation structure CN on the substrate surface. x Film: Among them, The flow rate of argon gas is controlled at 160sccm, the flow rate of nitrogen gas is switched from 50sccm to 20sccm every 6 minutes, and the high-power pulse power supply is changed synchronously with 1200V, 650V and the introduction of nitrogen gas; the current of the graphite target is 100A, the output power is changed synchronously with 12kW, 6.5KW and the introduction of nitrogen gas, and the bias voltage is always -70V; the cycle is repeated until the thickness of the diamond-like amorphous carbon coating reaches the target thickness.

2. A super lubricating graphene intercalation CN as claimed in claim 1 x The method for constructing a thin film is characterized by: The substrate is a single crystal silicon wafer with an orientation of 100.

3. A super lubricating graphene intercalation CN as claimed in claim 1 x The method for constructing a thin film is characterized by: The graphite center column target adopts a samarium cobalt magnet Sm2Co with a magnetic flux of 4000 17 .

4. A super lubricating graphene intercalation CN as claimed in claim 1 x The method for constructing a thin film is characterized by: The distance between the workpiece single crystal silicon wafer and the graphite central column target is adjusted to 11-15 cm.

5. A super lubricating graphene intercalation CN as claimed in claim 1 x The method for constructing a thin film is characterized by: During the entire process, the rotation speed of the graphite target and the work stand is 0.114 m / s.

6. A super lubricating graphene intercalation CN as claimed in claim 1 x The method for constructing a thin film is characterized by: The prepared super-lubricating graphene intercalation CN x In the film, the nitrogen doping amount is not less than 10.0 wt%, the carbon content is not less than 87.81 wt%, sp 3 The carbon content of the structure is at least 82 at%.