Amorphous / crystalline phase coexisting photocatalyst and its preparation method and application
By regulating the ratio of soluble niobium salt to water and the hydrothermal reaction temperature, a niobium pentoxide mesoporous photocatalyst with coexisting amorphous/crystalline phases was synthesized, which solved the problems of low catalytic activity and poor selectivity of existing photocatalysts and achieved high efficiency. Excellent CO2 reduction CH4 performance and simple preparation process.
Patent Information
- Application Number
- CN202310242043.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-14
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-03-14
AI Technical Summary
Existing photocatalysts have low catalytic activity in photocatalytic CO2 reduction of CH4, poor product selectivity, complicated preparation processes, and difficult to control catalytic performance.
By regulating the ratio of soluble niobium salt to water and the hydrothermal reaction temperature, a niobium pentoxide mesoporous photocatalyst with coexisting amorphous/crystalline phases was synthesized, and the morphology and surface interface properties of niobium oxide were controlled to improve its photocatalytic performance.
It achieves high photocatalytic performance and selectivity, simplifies the preparation process, reduces equipment requirements and harmful by-products, and improves the selectivity and efficiency of CO2 reduction of CH4.
Smart Images

Figure CN117599772B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photocatalytic materials, and in particular relates to a photocatalyst with coexistence of amorphous / crystalline phases and a preparation method and application thereof. Background Art
[0002] Nowadays, the global environmental and energy crises caused by the massive consumption of fossil fuels and the continuous increase in carbon dioxide emissions are becoming increasingly prominent. Photocatalytic reduction of carbon dioxide (CO2) is considered to be a promising sustainable energy conversion method that is expected to achieve carbon cycling. It can effectively convert CO2 gas into renewable fuels (such as CH4, CO, CH3OH, HCOOH or other high-value-added compounds) while alleviating the energy crisis and global warming problems. It is generally believed that catalysts play a decisive role in the photocatalytic performance of CO2 photoreduction by controlling the absorption and utilization of light, the activation of reactants and the reaction pathway. To date, various photocatalysts have been developed to reduce CO2 to renewable hydrocarbon fuels under mild conditions by mimicking efficient photosynthesis. However, selectivity and conversion efficiency remain a great challenge. It is necessary to develop efficient photocatalytic materials with strong light absorption ability, small CO2 activation energy barrier and high selectivity for the generation of non-toxic CH4.
[0003] The metal oxide niobium pentoxide (Nb2O5) is a common semiconductor material with the advantages of safety, non-toxicity, and good chemical stability. It is widely used in many fields including photocatalysis, gas sensors, traditional acid catalysis, electrochromism, field emission displays, and microelectronics. In the field of photocatalysis, the application of Nb2O5 is currently mainly concentrated in environmental remediation, such as photocatalytic degradation of organic pollutants. There are few reports on the use of Nb2O5 to photocatalytically reduce CO2 to prepare CH4 and other hydrocarbon fuels, with low photocatalytic activity and poor product selectivity. On the one hand, this is determined by its band structure: the band gap is wide (Eg~3.4eV), it can only adsorb and utilize visible light, the conduction band position is low, and the reduction ability of photogenerated electrons is poor; on the other hand, it is difficult to adsorb and activate CO2 molecules due to the lack of sufficient active sites.
[0004] Amorphous inorganic semiconductors have attracted increasing attention due to their unique electrical and optical properties arising from their inherent disordered structure and thermodynamic metastable state. Although amorphous semiconductor materials were reported to be inefficient photocatalysts in the early days, researchers have found that the coexistence of crystalline and amorphous phases plays an important role in the photocatalytic performance of the catalyst. Therefore, constructing a mesoporous niobium pentoxide photocatalyst with coexistence of amorphous / crystalline phases is expected to obtain ideal photocatalytic reduction of CO2 activity and selectivity for directional generation of CH4. However, the preparation of crystalline / amorphous photocatalysts usually requires complex processes, such as acid treatment of the catalyst surface and reduction with H2 at high temperature. Therefore, it is necessary to develop a simple method to prepare a mesoporous niobium pentoxide photocatalyst with coexistence of amorphous / crystalline phases with high photocatalytic performance and selectivity. Summary of the invention
[0005] The purpose of the present invention is to provide a photocatalyst with coexistence of amorphous / crystalline phases and a preparation method and application thereof, in view of the problem of complex existing photocatalyst preparation processes, and to synthesize a mesoporous niobium pentoxide photocatalyst with coexistence of amorphous / crystalline phases by regulating the ratio of soluble niobium salt to water and the hydrothermal reaction temperature, regulating the hydrolysis rate of the soluble niobium salt and the nucleation and growth rates of niobium pentoxide, and further regulating the morphology and surface and interface properties of niobium oxide to improve the catalytic performance of the photocatalyst.
[0006] In order to achieve the above purpose, the technical solution adopted in this application is:
[0007] A method for preparing a photocatalyst with coexistence of amorphous / crystalline phases comprises the following steps: using a soluble niobium salt as a precursor, adding water and reacting by a hydrothermal method, and after the reaction is completed, washing, drying to constant weight and grinding to obtain a mesoporous photocatalyst with coexistence of amorphous / crystalline phases.
[0008] Preferably, the soluble niobium salt is niobium pentachloride or niobium oxalate.
[0009] Preferably, the molar volume ratio of the soluble niobium salt to water is 0.5-2 mmol:30 mL.
[0010] Preferably, the temperature of the hydrothermal reaction is 140-180° C. and the time is 24 hours.
[0011] Preferably, the drying temperature is 60-90°C.
[0012] In addition, the present invention also provides a photocatalyst with coexistence of amorphous / crystalline phases prepared by the above preparation method.
[0013] The present invention also provides the use of the above-mentioned amorphous / crystalline phase coexisting photocatalyst in photocatalysis, wherein the photocatalyst selectively reduces CO2 to produce CH4.
[0014] Compared with the prior art, the present invention has the following beneficial effects:
[0015] (1) The present invention provides a simple method for preparing an amorphous / crystalline coexisting niobium pentoxide mesoporous photocatalyst with high photocatalytic performance and selectivity. The amorphous / crystalline coexisting niobium pentoxide mesoporous photocatalyst is synthesized by regulating the ratio of soluble niobium salt to water and the hydrothermal reaction temperature, regulating the hydrolysis rate of the soluble niobium salt and the nucleation and growth rates of niobium pentoxide, and then regulating the morphology and surface and interface properties of niobium oxide to improve the catalytic performance of the photocatalyst.
[0016] (2) The photocatalyst prepared by the present invention has a simple preparation process, short time consumption, easy operation, no need for strict equipment, no harmful or toxic by-products, is environmentally friendly, has abundant and easily available raw materials, and relatively safe experimental conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 X-ray diffraction pattern of the photocatalyst with coexistence of amorphous / crystalline phases constructed for the present invention;
[0018] Figure 2 An infrared spectrum of a photocatalyst with coexistence of amorphous / crystalline phases constructed for the present invention;
[0019] Figure 3 Transmission electron microscopy image of the photocatalyst with coexistence of amorphous / crystalline phases constructed for the present invention;
[0020] Figure 4 A high-magnification transmission electron microscopy image of a photocatalyst with coexistence of amorphous / crystalline phases constructed for the present invention;
[0021] Figure 5 A nitrogen adsorption-desorption isotherm of a photocatalyst with coexistence of amorphous / crystalline phases is constructed for the present invention;
[0022] Figure 6 The BJH pore size distribution curve of the photocatalyst with coexistence of amorphous / crystalline phases is constructed for the present invention;
[0023] Figure 7 A CO2 adsorption curve of a photocatalyst with coexistence of amorphous / crystalline phases is constructed for the present invention;
[0024] Figure 8 The UV-visible absorption spectrum of the photocatalyst with coexistence of amorphous / crystalline phases is constructed for the present invention;
[0025] Fig. 9 The energy band width diagram calculated based on the UV-visible absorption spectrum of the catalyst with coexistence of amorphous / crystalline phases constructed for the present invention;
[0026] Fig.10A graph showing the relationship between the amount of CH4 produced by photocatalytic reduction of CO2 per unit mass of a photocatalyst with coexistence of amorphous / crystalline phases and the time of the photocatalyst is constructed for the present invention;
[0027] Fig.11 A graph showing the relationship between the amount of CO produced by photocatalytic reduction of CO2 per unit mass of a photocatalyst with coexisting amorphous / crystalline phases and the time of the photocatalyst is constructed for the present invention.
[0028] Fig.12 A selectivity data diagram for the photocatalytic reduction production of CH4 by a photocatalyst with coexisting amorphous / crystalline phases is constructed for the present invention. DETAILED DESCRIPTION
[0029] The following will combine the data in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] It should be noted that the professional terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specifically stated, the various raw materials, reagents, instruments and equipment used in the following embodiments of the present invention can be purchased from the market or prepared by existing methods.
[0031] Example 1
[0032] A method for preparing an amorphous niobium pentoxide photocatalyst comprises the following steps:
[0033] Weigh 1 mmol niobium pentachloride (NbCl5), dissolve it in 30 mL deionized water, and ultrasonically disperse it for 15 minutes to obtain a white uniform suspension, which is then transferred to a 50 mL high-pressure reactor, placed in an oven, heated to 160°C and subjected to hydrothermal reaction for 24 hours. After the hydrothermal reaction cools to room temperature, it is washed with water and alcohol several times, dried at 80°C overnight, and ground to obtain a mesoporous niobium pentoxide photocatalyst with coexistence of amorphous / crystalline phases, named NBO-1.
[0034] Example 2
[0035] A method for preparing an amorphous niobium pentoxide photocatalyst comprises the following steps:
[0036] Weigh 1 mmol niobium pentachloride (NbCl5), dissolve it in 30 mL deionized water, and ultrasonically disperse it for 15 minutes to obtain a white uniform suspension, which is then transferred to a 50 mL high-pressure reactor, placed in an oven, heated to 140°C and subjected to hydrothermal reaction for 24 hours. After the hydrothermal reaction cools to room temperature, it is washed with water and alcohol several times, dried at 80°C overnight, and ground to obtain a mesoporous niobium pentoxide photocatalyst with coexistence of amorphous / crystalline phases, named NBO-2.
[0037] Example 3
[0038] A method for preparing an amorphous niobium pentoxide photocatalyst comprises the following steps:
[0039] Weigh 1 mmol niobium pentachloride (NbCl5), dissolve it in 30 mL deionized water, and ultrasonically disperse it for 15 minutes to obtain a white uniform suspension, which is then transferred to a 50 mL high-pressure reactor, placed in an oven, heated to 180°C and subjected to hydrothermal reaction for 24 hours. After the hydrothermal reaction cools to room temperature, it is washed with water and alcohol several times, dried at 80°C overnight, and ground to obtain a mesoporous niobium pentoxide photocatalyst with coexistence of amorphous / crystalline phases, named NBO-3.
[0040] Example 4
[0041] A method for preparing a Nb2O5 photocatalyst comprises the following steps:
[0042] Weigh 1 mmol of niobium oxalate (C 10 H5B 20 ), dissolved in 30 mL of deionized water, ultrasonically dispersed for 15 min to obtain a white uniform suspension, which was then transferred to a 50 mL high-pressure reactor, placed in an oven, heated to 160 ° C and subjected to hydrothermal reaction for 24 h. After the hydrothermal reaction cooled to room temperature, it was washed with water and alcohol several times, dried at 80 ° C overnight, and ground to obtain amorphous / crystalline phase coexisting niobium pentoxide mesoporous photocatalyst, named NBO-4.
[0043] Comparative Example 1
[0044] A method for preparing a Nb2O5 photocatalyst comprises the following steps:
[0045] S1. Weigh 1 mmol of niobium pentachloride (NbCl5), dissolve it in 30 mL of deionized water, and perform ultrasonic dispersion for 15 min to obtain a white uniform suspension. Then transfer it to a 50 mL high-pressure reactor, put it in an oven, heat it to 160 ° C, and perform hydrothermal reaction for 24 h. After the hydrothermal reaction cools to room temperature, wash it with water and alcohol several times, dry it at 80 ° C overnight, and grind it to obtain a mesoporous photocatalyst with coexistence of amorphous / crystalline phases of niobium pentoxide;
[0046] S2. Place Nb2O5 powder in a porcelain boat, then put it into a tubular furnace, heat it to 400°C at a rate of 5°C / min in an air atmosphere, calcine it for 2 hours, and then cool it to room temperature to obtain a sample prepared by high-temperature calcination, named NBO-400.
[0047] Comparative Example 2
[0048] A method for preparing a Nb2O5 photocatalyst comprises the following steps:
[0049] S1. Weigh 1 mmol of niobium pentachloride (NbCl5), dissolve it in 30 mL of deionized water, and perform ultrasonic dispersion for 15 min to obtain a white uniform suspension. Then transfer it to a 50 mL high-pressure reactor, put it in an oven, heat it to 160 ° C, and perform hydrothermal reaction for 24 h. After the hydrothermal reaction cools to room temperature, wash it with water and alcohol several times, dry it at 80 ° C overnight, and grind it to obtain a mesoporous photocatalyst with coexistence of amorphous / crystalline phases of niobium pentoxide;
[0050] S2. Place Nb2O5 powder in a porcelain boat, then put it into a tubular furnace, heat it to 600°C at a rate of 5°C / min in an air atmosphere, calcine it for 2 hours, and then cool it to room temperature to obtain a sample prepared by high-temperature calcination, named NBO-600.
[0051] Figure 1 The X-ray diffraction pattern (XRD) of the amorphous / crystalline coexisting niobium pentoxide mesoporous photocatalyst constructed by the present invention is shown in FIG. Figure 1 As shown, after calcination at 600℃, Comparative Example 2 NBO-600 has a sharp XRD diffraction peak. After comparison with the XRD standard card (JCPDS: 27-1003), we believe that Comparative Example 2 NBO-600 is hexagonal Nb2O5. The one-step hydrothermal preparation of Nb2O5 (Example 1) has poor crystallinity, but its XRD spectrum has a bulge between 20° and 30° that basically corresponds to hexagonal Nb2O5. Therefore, we believe that it is poorly crystallized Nb2O5, which can be explained as hydrated niobium pentoxide. After calcination at 400℃, the crystallinity of Comparative Example 1 NBO-400 has no obvious change compared with that before calcination.
[0052] Figure 2 The infrared spectrum (IR) of the amorphous / crystalline coexisting niobium pentoxide mesoporous photocatalyst constructed by the present invention. Figure 2 As shown, at 3100~3500cm -1The broad vibration peak in the range is related to the vibration stretching peak of OH in the H2O molecule. The one-step hydrothermal prepared Nb2O5 (Example 1) has the strongest vibration stretching peak of OH. After calcination at 400°C, the vibration stretching peak of OH in Comparative Example 1 NBO-400 is significantly weakened, which is caused by the loss of water. After high-temperature calcination at 600°C, the vibration stretching peak of OH in Comparative Example 2 NBO-600 completely disappears, indicating that the adsorbed H2O and structural H2O are all lost.
[0053] Figure 3 The transmission electron microscope (TEM) image of the amorphous / crystalline coexisting niobium pentoxide mesoporous photocatalyst constructed by the present invention is shown in FIG. Figure 3 The NBO-1 in Example 1 shown above all presents a porous morphology with nanoparticles stacked.
[0054] Figure 4 This is a high magnification transmission electron microscopy (HRTEM) image of the amorphous / crystalline coexisting niobium pentoxide mesoporous photocatalyst constructed by the present invention. Figure 4 The shown example 1 NBO-1 has certain lattice fringes, and the lattice fringes are surrounded by amorphous components, indicating that the prepared material is a material in which amorphous / crystalline phases coexist.
[0055] Figure 5 The nitrogen adsorption-desorption isotherm of the amorphous / crystalline coexisting niobium pentoxide mesoporous photocatalyst was constructed for the present invention. Figure 5 As shown, NBO-1 in Example 1 presents a Type IV N2 adsorption curve with a specific surface area of 355 m 2 / g.
[0056] Figure 6 The BJH pore size distribution curve of the amorphous / crystalline coexisting niobium pentoxide mesoporous photocatalyst is constructed for the present invention. Figure 6 As shown, Example 1 NBO-1 is a mesoporous material with a pore size of less than 4 nm.
[0057] Figure 7 The CO2 adsorption curve of the amorphous / crystalline coexisting niobium pentoxide mesoporous photocatalyst was constructed for the present invention. Figure 7 As shown, Example 1 NBO-1 has a higher CO2 adsorption capacity. After high-temperature calcination, as the calcination temperature increases, the CO2 adsorption capacity of Comparative Example 1 NBO-400 and Comparative Example 2 NBO-600 gradually decreases.
[0058] Figure 8 The UV-visible absorption spectrum (DRS) of the amorphous / crystalline coexisting niobium pentoxide mesoporous photocatalyst was constructed for the present invention. Figure 8As shown, Example 1 NBO-1, Comparative Example 1 NBO-400 and Comparative Example 2 NBO-600 have strong light absorption mainly in the ultraviolet region. In this region, Example 1 NBO-1 exhibits the strongest light absorption intensity.
[0059] Fig. 9 The energy band width diagram of the amorphous / crystalline coexisting niobium pentoxide mesoporous photocatalyst constructed for the present invention is calculated based on the UV-visible absorption spectrum (DRS). Fig. 9 As shown, Example 1 NBO-1 has the narrowest bandgap, that is, the widest visible light absorption range.
[0060] The Nb2O5 catalysts prepared in Examples 1-4 and Comparative Examples 1-2 were subjected to photocatalytic research, and the photocatalytic CO2 test process was as follows:
[0061] 5mL deionized water (providing the water vapor required for reducing carbon dioxide) is added to the reactor, and 50mg sample is evenly spread on the glass plate in the glass reactor. Before illumination, the reactor is filled with Ar gas, and 1mL high-purity CO2 gas is injected into the reactor. Subsequently, a 300W xenon lamp is used to irradiate from the top of the reactor to react. Then, 1mL gas is extracted from the reactor every 30min and injected into a gas chromatograph (Zhejiang Fu Li, GC9790II). The amount of the substance of the reduction product CH4 and CO is determined respectively using the external standard method, and the selectivity of the catalyst photocatalytic reduction production CH4 is calculated by comparison.
[0062] Fig.10 The present invention constructs a graph showing the relationship between the amount of CH4 produced by photocatalytic reduction of CO2 per unit mass of amorphous / crystalline coexisting niobium pentoxide mesoporous photocatalyst and the time. Fig.10 As shown, Example 1 NBO-1 exhibits the best photocatalytic activity.
[0063] Fig.11 The present invention constructs a graph showing the relationship between the amount of CO produced by photocatalytic reduction of CO2 per unit mass of amorphous / crystalline phase coexisting niobium pentoxide mesoporous photocatalyst and the time. Fig.11 As shown, Example 4 NBO-4 exhibits the best photocatalytic activity.
[0064] Fig.12 The selectivity data diagram of CH4 produced by photocatalytic reduction of mesoporous niobium pentoxide photocatalyst with coexistence of amorphous / crystalline phases is constructed for the present invention (calculated based on the amount of CH4 and CO produced per unit catalyst per unit time). Fig.12 As shown, Example 1 NBO-1 exhibits the highest selectivity for photocatalytic reduction of CO2 to produce CH4, reaching 85.7%.
[0065] It should be noted that when the present invention involves a numerical range, it should be understood that the two endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as those in the embodiments, in order to avoid redundancy, the present invention describes a preferred embodiment. Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they know the basic creative concept. Therefore, the attached claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0066] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. Application of a photocatalyst with coexistence of amorphous / crystalline phases in photocatalysis, characterized in that: The photocatalyst selectively reduces CO2 to prepare CH4. The preparation method of the photocatalyst comprises the following steps: using a soluble niobium salt as a precursor, adding water and reacting by a hydrothermal method, washing, drying to constant weight and grinding after the reaction to obtain a mesoporous photocatalyst with coexistence of amorphous / crystalline phases; The temperature of the hydrothermal reaction is 140-160°C and the time is 24 h.
2. The use of the catalyst with coexistence of amorphous / crystalline phases according to claim 1 in photocatalysis, characterized in that: The soluble niobium salt is niobium pentachloride or niobium oxalate.
3. The use of the amorphous / crystalline coexisting photocatalyst according to claim 1 in photocatalysis, characterized in that: The molar volume ratio of the soluble niobium salt to water is 0.5-2 mmol:30 mL.
4. The use of the amorphous / crystalline phase coexisting photocatalyst according to claim 1 in photocatalysis, characterized in that: The drying temperature is 60-90°C.
Citation Information
Patent Citations
Novel Glycerol Dehydration Catalyst and Production Method Therefor
US20130303801A1