A high temperature sealing glass-ceramic and its preparation and application

By using specific component proportions and heat treatment technology in high-temperature sealing glass, a tight network structure is formed, which solves the problems of deterioration of electrical insulation and mismatch of thermal expansion coefficient at high temperatures, and achieves good sealing and high temperature with Kova Alloy Insulation.

CN117602838BActive Publication Date: 2024-11-19WUHAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311577896.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-22
Publication Date
2024-11-19
Estimated Expiration
2043-11-22

AI Technical Summary

Technical Problem

The electrical insulation of existing high-temperature sealing glass deteriorates at high temperatures, and the thermal expansion coefficient does not match the coval alloy, resulting in poor sealing and cracking problems.

Method used

The proportions of components of 55-65 parts SiO2, 8-15 parts Al2O3, 10-20 parts B2O3, 4-10 parts ZnO, 4-10 parts R2O, 4-10 parts CaO, 4-10 parts ZrO2 were adopted by melting, Homogenization, annealing, nucleation and crystallization treatment were made to prepare high-temperature sealed microcrystalline glass to form the main crystal phase of Al0.52Zr0.48O1.74 and ZrO2, increasing the tightness and resistivity of the network structure.

Benefits of technology

Maintain good insulation performance and moderate expansion coefficient at high temperatures, match the thermal expansion coefficient of KVA alloy, improve sealing strength and insulation, and extend the temperature range of use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117602838B_ABST
    Figure CN117602838B_ABST
Patent Text Reader

Abstract

The present invention discloses a high-temperature sealing microcrystalline glass and its preparation and application, comprising the following components by mass: 55-65 parts of SiO2, 8-15 parts of Al2O3, 10-20 parts of B2O3, 4-10 parts of ZnO, 4-10 parts of R2O, 4-10 parts of CaO, and 4-10 parts of ZrO2; wherein R2O is one or more of Na2O and K2O; the obtained high-temperature sealing microcrystalline glass has a softening point greater than 600°C, a high matching degree with the thermal expansion coefficient of Kovar alloy, and a resistivity greater than 3.72×10 9 Ω·cm, the higher the resistivity, the better the insulation. The density of the high temperature sealing microcrystalline glass of the present application is 2.39g / cm 3 ‑2.46g / cm 3 At high temperatures, the high-temperature sealing microcrystalline glass of the present application maintains a good matching seal with the Kovar alloy and has good insulation properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of glass products, and in particular to a high-temperature sealed microcrystalline glass and preparation and application thereof. Background Art

[0002] Sealing glass is a non-aging, temperature-resistant "glue" that has functions such as electrical insulation, physical support, and signal transmission. It is an intermediate transition material for achieving reliable connections between metals, ceramics, other glasses, and composite materials. Compared with general sealing technologies, sealing glass has obvious advantages, mainly manifested in good mechanical properties and high airtightness.

[0003] Sealing glass is divided into low-temperature sealing glass and high-temperature sealing glass according to the sealing temperature. Low-temperature sealing glass is also called low-melting-point sealing glass. Its melting point is significantly lower than that of ordinary glass, generally below 600°C. High-temperature sealing glass is glass that is sealed at a higher temperature (sealing temperature above 800°C). The glass transition temperature, softening temperature and melting point of high-temperature sealing glass are higher. Kovar alloy is an Fe-Ni-Co alloy with Fe as the main matrix element. Its expansion coefficient is similar to that of silicon boron hard glass, about 50±5×10 -7 ℃ -1 Therefore, Kovar alloy and glass sealing are widely used in electronic packaging fields such as incandescent lamps, electron tubes, and semiconductor shells. The glass used for Kovar alloy sealing must have the characteristics of insulation, high temperature resistance, and can still play a sealing role at high temperatures. In the relevant technology, the sealing glass used for Kovar alloy is mostly a glass with a thermal expansion coefficient of 3-5×10 -6 ℃ -1 SiO 2 -B 2 O 3 glass system (7070, Corning). However, as the operating temperature increases from 25°C to 350°C, the volume resistivity of the sealing glass increases from 10 12 Ω·cm is reduced to 10 7 Ω·cm, so the maximum operating temperature of the sealing glass is limited to 350℃. In addition, when the operating temperature is higher than the glass transition temperature Tg, the alkali metal or alkaline earth metal ions migrate more easily in the glass network structure, and the resistivity of the sealing glass decreases rapidly, resulting in deterioration of electrical insulation. This limits the operating temperature of the sealing glass device and has an adverse effect on its electrical properties. Other high-temperature sealing glasses, such as La 2 O 3 -BaO-SiO 2 The system high temperature sealing glass still has 10 11 The resistivity is 10 Ω·cm, and it still has a resistance of 10 when it continues to rise to 600℃. 9The resistivity of Ω·cm is good for insulation. However, its thermal expansion coefficient is between 12.48-13.18×10 -6 ℃ -1 , the expansion coefficient of SS is very different from that of Kovar alloy, and it cannot be used for matching sealing of Kovar alloy, otherwise it will cause cracking and other problems.

[0004] Therefore, it is necessary to provide a sealing glass that can maintain the insulating properties of glass at high temperatures and has a moderate expansion coefficient to achieve sealing with Kovar alloy. Summary of the invention

[0005] In view of this, the present application provides a high-temperature sealed microcrystalline glass and its preparation and application, to solve the problem of how to achieve good sealing and good insulation between the sealing glass and the Kovar alloy at high temperature.

[0006] In order to achieve the above technical objectives, this application adopts the following technical solutions:

[0007] In a first aspect, the present application provides a high temperature sealed microcrystalline glass, comprising the following components by mass: 55-65 parts SiO 2 , 8-15 parts Al 2 O 3 10-20 portions B 2 O 3 , 4-10 parts ZnO, 4-10 parts R 2 O, 4-10 parts CaO, 4-10 parts ZrO 2 ; where R 2 O is Na 2 O.K 2 One or more of O.

[0008] Preferably, the main crystalline phase is Al 0.52 Zr 0.48 O 1.74 and ZrO 2 , the crystallinity of the main crystalline phase is 5-19%.

[0009] More preferably, R 2 O is K 2 O.

[0010] In a second aspect, the present application provides a method for preparing a high-temperature sealed microcrystalline glass, comprising the following steps:

[0011] S1. Powdered SiO 2 、Al 2 O 3 , B 2 O 3 、ZnO、R 2 O, CaO, ZrO 2The mixture is uniformly mixed, melted, homogenized and clarified, and then formed, and then annealed to obtain the basic glass;

[0012] S2. The base glass is subjected to nucleation and crystallization heat treatments in sequence to obtain high-temperature sealed microcrystalline glass.

[0013] Preferably, in step S1, the melting temperature is 1500-1600° C., and the melting time is 2-4 hours.

[0014] Preferably, in step S1, the annealing temperature is 580-650° C., and the annealing time is 1-3 h.

[0015] Preferably, in step S2, the nucleation temperature is 850-950° C., and the nucleation time is 0.5-3 h.

[0016] Preferably, in step S2, the crystallization temperature is 1100-1350° C., and the crystallization time is 0.5-3 h.

[0017] In a third aspect, the present application provides an application of high-temperature sealing microcrystalline glass in Kovar alloy sealing.

[0018] Preferably, the sealing temperature is 800-1025°C.

[0019] The beneficial effects of this application are as follows:

[0020] Under the composition ratio of the present application, a high temperature sealed microcrystalline glass is obtained by heat treatment. After the heat treatment, the glass undergoes different degrees of crystallization, and the main crystal phase precipitated is Al 0.52 Zr 0.48 O 1.74 (PDF#53-0294) and ZrO 2 (PDF#37-1484), the crystallinity of the main crystalline phase is about 5-19%, the two main crystalline phases have high melting points, high resistivity and low expansion coefficient; at the same time, in the process of forming high-temperature sealing microcrystalline glass, the boron oxide triangle [BO 3 ] to the boron-oxygen tetrahedron [BO 4 ] transformation, resulting in the transformation from part of the two-dimensional layered structure to the three-dimensional frame structure, thereby increasing the network structure to make the structure compact, thereby achieving the effect of reducing the thermal expansion coefficient and increasing the resistivity; furthermore, the crystals precipitated in the present application still exist under high temperature conditions and have a greater hindering effect on the migration of alkali metal ions, so that the resistivity remains relatively stable, that is, when alkali metals as carriers move in a directional manner, on the one hand, they will be affected by the resistance of the main crystalline phase, and on the other hand, they will be limited by the range of the three-dimensional frame structure, resulting in a large resistivity of the high-temperature sealed microcrystalline glass, thereby further increasing the insulation of the high-temperature sealed microcrystalline glass.

[0021] The high temperature sealing microcrystalline glass obtained in the present application has a softening point temperature greater than 600°C, and a thermal expansion coefficient within the temperature range of 20°C-600°C of (47±10)×10 7 ℃ -1 In this application, Al 2 O 3 With ZrO 2 Under the dosage limit, Al can enter ZrO 2 lattice, forming Al 0.52 Zr 0.48 O 1.74 , if Al 2 O 3 Excessive use of Al 0.52 Zr 0.48 O 1.74 The crystal phase content decreases, ZrO 2 The crystal phase content increases and the overall crystallization degree decreases. The room temperature resistivity of the sealed microcrystalline glass of the present application is between 1.58×10 12 -8.01×10 14 Ω·cm, the resistivity is always greater than 3.72×10 9 Ω·cm, the higher the resistivity, the better the insulation. And the density of the sealed microcrystalline glass of the present application is 2.39g / cm 3 -2.46g / cm 3 At high temperatures, the high-temperature sealing microcrystalline glass of the present application maintains a good matching seal with the Kovar alloy and has good insulation properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 X-ray test results of the glass-ceramics of Examples 1-5;

[0023] Figure 2 The scanning electron microscope test results of the glass-ceramics of Example 4;

[0024] Figure 3 These are the X-ray test results of the glass-ceramics of Comparative Example 1-2. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0026] The present application provides a high-temperature sealed microcrystalline glass, comprising the following components in mass fractions: 55-65 parts SiO 2 , 8-15 parts Al 2 O 310-20 portions B 2 O 3 , 4-10 parts ZnO, 4-10 parts R 2 O, 4-10 parts CaO, 4-10 parts ZrO 2 ; where R 2 O is Na 2 O.K 2 One or more of O. Al of this application 2 O 3 With ZrO 2 Under the dosage limit, the tetragonal Al 0.52 Zr 0.48 O 1.74 and monoclinic ZrO 2 During the cooling process, ZrO 2 It will transform from tetragonal phase to monoclinic phase. At high temperature, Al in the system can enter ZrO 2 , forming a tetragonal Al 0.52 Zr 0.48 O 1.74 , if Al 2 O 3 Excessive use of Al 0.52 Zr 0.48 O 1.74 The crystal phase content decreases, ZrO 2 The crystal content increases and the overall crystallization degree decreases. 2 O all use K 2 O crystallization effect is better, but using Na 2 The sealing temperature is lower at O.

[0027] The main crystalline phase of the high temperature sealing glass-ceramics of the present application is Al 0.52 Zr 0.48 O 1.74 and ZrO 2 , the crystallinity of the main crystalline phase is 5-19%.

[0028] The present application provides a method for preparing a high-temperature sealed microcrystalline glass, comprising the following steps:

[0029] S1. Powdered SiO 2 、Al 2 O 3 , B 2 O 3 、ZnO、R 2 O, CaO, ZrO 2 The mixture is uniformly mixed, melted, homogenized and clarified, and then formed, and then annealed to obtain the basic glass;

[0030] S2. The base glass is subjected to nucleation and crystallization heat treatments in sequence to obtain high-temperature sealed microcrystalline glass.

[0031] The high-resistance high-temperature sealing glass-ceramic of the present application is SiO 2 As the glass network skeleton, by adjusting the relative content of each component, sufficient free oxygen is provided in the glass structure. Under a certain total amount, ZnO, R 2 The increase of O content will increase the free oxygen. At the same time, when the non-bridging oxygen increases, the boron oxygen triangle [BO 3 ] to the boron-oxygen tetrahedron [BO 4 ] transformation, resulting in the transformation from a partial two-dimensional layered structure to a three-dimensional frame structure, thereby increasing the network structure and making the structure compact, thereby achieving the effect of reducing the thermal expansion coefficient and increasing the resistivity. In addition, due to the three-dimensional frame structure of the present application, the space for directional movement of carriers can be limited, reducing conductivity. In some embodiments, using a material that is relatively thinner than Na + K with a larger radius + As a carrier, the greater the resistance it faces during movement, the worse the conductivity and the higher the resistivity.

[0032] In this application, ZrO 2 As a crystal nucleating agent, under the component definition of this application, when the crystal nucleating agent is ZrO 2 Al is most likely to precipitate when 0.52 Zr 0.48 O 1.74 and ZrO 2 When replacing the nucleating agent such as TiO 2 After that, only other crystal phases can be precipitated. The preparation temperature mainly affects the number and size of the precipitated crystals.

[0033] By adjusting the content of the network exosomes through appropriate component ratios, the content of free oxygen can be changed, which can change the optimal crystallization temperature, resulting in different degrees of crystallization under the same heat treatment system. 0.52 Zr 0.48 O 1.74 (PDF#53-0294) and ZrO 2 (PDF#37-1484), the crystallinity is about 5-19%. ZrO at room temperature 2 (PDF#37-1484) has a monoclinic phase structure, a space group of P21 / c, lattice constants of a=5.142, b=5.206, c=5.313, β=99°18, is chemically inactive, and has the properties of high melting point, high resistivity, high refractive index and low thermal expansion coefficient. Al 0.52 Zr 0.48 O 1.74 (PDF#53-0294) As Al atoms enter the tetragonal ZrO phase at high temperatures2 The lattice replaces the position of some Zr atoms to form a uniform solid solution, which maintains the tetragonal phase structure at room temperature while also having the characteristics of high resistivity and low thermal expansion coefficient. The main crystal of this application has a large resistance to carriers, which will make the volume resistivity of the material larger. Coupled with the high resistivity characteristics of the two crystals themselves, the material has excellent electrical insulation properties from room temperature to 600°C, thereby greatly improving the application temperature range of the material. It is worth noting that the reason why the main crystal of this application has a large resistance to carriers is that, first, the two crystal phases generated themselves have high electrical insulation properties, and secondly, the higher the crystallinity and the more crystals there are, the stronger the resistance to ion movement and the greater the resistivity. The microcrystalline glass used for high-temperature sealing in this application has high-temperature insulation properties in order to better meet the requirements that the sealed device can work normally in a high-temperature environment.

[0034] In step S1, the melting temperature is 1500-1600°C and the melting time is 2-4h. If the melting temperature is too low, the raw material cannot be melted and cannot be formed.

[0035] In step S1, the annealing temperature is 580-650°C and the annealing time is 1-3h. If the annealing temperature is too low, the thermal stress cannot be eliminated and cracking is likely to occur.

[0036] In step S2, the nucleation temperature is 850-950°C, and the nucleation time is 0.5-3h. Too high or too low a nucleation temperature will reduce the number of crystal nuclei.

[0037] In step S2, the crystallization temperature is 1100-1350°C and the crystallization time is 0.5-3h. If the crystallization temperature is too low, the size of the crystal is small; if the crystallization temperature is too high, the grain size increases, or even secondary recrystallization / remelting occurs.

[0038] The softening point of the high temperature sealing microcrystalline glass obtained in the present application is greater than 600°C, and the thermal expansion coefficient in the temperature range of 20°C-600°C is (47±10)×10 7 ℃ -1 The thermal expansion coefficient of Kovar alloy is highly matched, and its room temperature resistivity is between 1.58×10 12 -8.01×10 14 Ω·cm, and the resistivity is always greater than 3.72×10 9 Ω·cm, the higher the resistivity, the better the insulation. The density of the high temperature sealing microcrystalline glass of the present application is 2.39g / cm 3 -2.46g / cm 3 At high temperatures, the high-temperature sealing microcrystalline glass of the present application maintains a good matching seal with the Kovar alloy and has good insulation properties.

[0039] The present application provides an application of high-temperature sealed microcrystalline glass in Kovar alloy sealing, the sealing temperature is 800-1025°C. It is worth noting that the sealing temperature should be slightly higher than the softening temperature of the glass material because the glass needs to have a certain fluidity during sealing.

[0040] The present application is further described below through specific implementation methods.

[0041] The raw materials used in the examples of the present invention are all chemically pure raw materials, but trace amounts of inevitable impurities are allowed; a high-temperature melting furnace is used for glass melting; a crystallization furnace is used for crystallization; and annealing is performed in an annealing furnace.

[0042] Example 1

[0043] A high-temperature sealing microcrystalline glass, comprising the following components by mass: 58 parts SiO 2 , 9 parts Al 2 O 3 , 13 copies B 2 O 3 , 5 parts ZnO, 5 parts Na 2 O, 5 parts CaO, 5 parts ZrO 2 , the sum of the mass proportions of each component is 100%.

[0044] The method for preparing high temperature sealed glass-ceramics comprises the following steps:

[0045] S1. Raw materials are weighed according to the amounts of the above components to prepare a basic glass batch material. The batch material is melted and kept at 1600°C for 3 hours. After high-temperature homogenization and clarification, a glass liquid is obtained. After the glass liquid is formed by a casting method, it enters an annealing furnace and is kept at 620°C for 2 hours for annealing treatment to obtain a basic glass.

[0046] S2. The base glass is subjected to a nucleation treatment by being kept at 900°C for 0.5h, and then subjected to a crystallization heat treatment by being kept at 1300°C for 0.5h, and then cooled in the furnace to obtain a high-temperature sealed microcrystalline glass, which is then cut, polished, and subjected to subsequent performance tests.

[0047] The main crystalline phase of the high temperature sealing glass-ceramics obtained in this embodiment is Al 0.52 Zr 0.48 O 1.74 (PDF#53-0294) and ZrO 2 (PDF#37-1484), the crystallinity is about 5-7%; the test results of microcrystalline glass X-ray are as follows Figure 1 As shown; the softening point is 630℃; the thermal expansion coefficient in the temperature range of 20℃-600℃ is 52.3×10 7 ℃ -1 ; Density about 2.395g / cm 3; Room temperature resistivity is about 1.58×10 12 Ω·cm; Sealing temperature range 900℃-950℃.

[0048] Example 2

[0049] A high-temperature sealing microcrystalline glass, comprising the following components in parts by mass: 55 parts SiO 2 , 11.5 parts Al 2 O 3 10 copies of B 2 O 3 , 6 parts ZnO, 1.98 parts Na 2 O, 3.02 parts K 2 O, 7 parts CaO, 5 parts ZrO 2 ; The sum of the mass percentages of each component is 100%.

[0050] The method for preparing high temperature sealed glass-ceramics comprises the following steps:

[0051] S1. Raw materials are weighed according to the amounts of the above components to prepare a basic glass batch material. The batch material is melted and kept at 1600°C for 3 hours. After high-temperature homogenization and clarification, a glass liquid is obtained. After the glass liquid is formed by a casting method, it enters an annealing furnace and is kept at 620°C for 2 hours for annealing treatment to obtain a basic glass.

[0052] S2. The base glass is subjected to a nucleation treatment by being kept at 900°C for 0.5h, and then subjected to a crystallization heat treatment by being kept at 1200°C for 0.5h, and then cooled in the furnace to obtain a high-temperature sealed microcrystalline glass, which is then cut, polished, and subjected to subsequent performance tests.

[0053] The main crystalline phase of the high temperature sealing glass-ceramics obtained in this embodiment is Al 0.52 Zr 0.48 O 1.74 (PDF#53-0294) and ZrO 2 (PDF#37-1484), the crystallinity is about 10-12%, and the test results of microcrystalline glass X-ray are as follows Figure 1 As shown; the softening point is 692℃; the thermal expansion coefficient in the temperature range of 20℃-600℃ is 46.7×10 7 ℃ -1 ; Density about 2.431g / cm 3 ; Room temperature resistivity is about 1.51×10 13 Ω·cm; Sealing temperature range 900℃-975℃.

[0054] Example 3

[0055] A high-temperature sealing microcrystalline glass, comprising the following components in parts by mass: 55 parts SiO 2 , 11.5 parts Al2 O 3 10 copies of B 2 O 3 , 6 parts ZnO, 1.98 parts Na 2 O, 3.02 parts K 2 O, 7 parts CaO, 5 parts ZrO 2 ; The sum of the mass percentages of each component is 100%.

[0056] The method for preparing high temperature sealed glass-ceramics comprises the following steps:

[0057] S1. Raw materials are weighed according to the amounts of the above components to prepare a basic glass batch material. The batch material is melted and kept at 1600°C for 3 hours. After high-temperature homogenization and clarification, a glass liquid is obtained. After the glass liquid is formed by a casting method, it enters an annealing furnace and is kept at 620°C for 2 hours for annealing treatment to obtain a basic glass.

[0058] S2. The base glass is subjected to a nucleation treatment by being kept at 900°C for 0.5h, and then subjected to a crystallization heat treatment by being kept at 1300°C for 0.5h, and then cooled in the furnace to obtain a high-temperature sealed microcrystalline glass, which is then cut, polished, and subjected to subsequent performance tests.

[0059] The main crystalline phase of the high temperature sealing glass-ceramics obtained in this embodiment is Al 0.52 Zr 0.48 O 1.74 (PDF#53-0294) and ZrO 2 (PDF#37-1484), the crystallinity is about 15-18%, and the test results of microcrystalline glass X-ray are as follows Figure 1 As shown; the softening point is 696℃; the thermal expansion coefficient in the temperature range of 20℃-600℃ is 45.5×10 7 ℃ -1 ; Density about 2.449g / cm 3 ; Room temperature resistivity is about 2.10×10 14 Ω·cm; Sealing temperature range 925℃-975℃.

[0060] Example 4

[0061] A high-temperature sealing microcrystalline glass, comprising the following components by mass: 56.5 parts SiO 2 , 11.5 parts Al 2 O 3 , 13 copies B 2 O 3 , 5 parts ZnO, 1.24 parts Na 2 O, 3.76 parts Na 2 O, 4 parts CaO, 5 parts ZrO 2 ; The sum of the mass percentages of each component is 100%.

[0062] The method for preparing high temperature sealed glass-ceramics comprises the following steps:

[0063] S1. Raw materials are weighed according to the amounts of the above components to prepare a basic glass batch material. The batch material is melted and kept at 1600°C for 3 hours. After high-temperature homogenization and clarification, a glass liquid is obtained. After the glass liquid is formed by a casting method, it enters an annealing furnace and is kept at 620°C for 2 hours for annealing treatment to obtain a basic glass.

[0064] S2. The base glass is subjected to a nucleation treatment at 900°C for 0.5h, followed by a crystallization heat treatment at 1300°C for 0.5h and then cooled in the furnace to obtain a high-temperature sealed microcrystalline glass, which is then cut, polished, and subjected to subsequent performance tests. The scanning electron microscope test results of the high-temperature sealed microcrystalline glass of this embodiment are as follows: Figure 2 shown.

[0065] The main crystalline phase of the high temperature sealing glass-ceramics obtained in this embodiment is Al 0.52 Zr 0.48 O 1.74 (PDF#53-0294) and ZrO 2 (PDF#37-1484), the crystallinity is about 16-19%, and the test results of microcrystalline glass X-ray are as follows Figure 1 As shown; the softening point is 743℃; the thermal expansion coefficient in the temperature range of 20℃-600℃ is 44.7×10 7 ℃ -1 ; Density about 2.448g / cm 3 ; Room temperature resistivity is about 7.10×10 14 Ω·cm; Sealing temperature range 925℃-975℃.

[0066] Example 5

[0067] A high-temperature sealing microcrystalline glass, comprising the following components by mass: 57.5 parts SiO 2 , 8.5 parts Al 2 O 3 15 B 2 O 3 , 4 parts ZnO, 5 parts K 2 O, 4 parts CaO, 6 parts ZrO 2 ; The sum of the mass percentages of each component is 100%.

[0068] The method for preparing high temperature sealed glass-ceramics comprises the following steps:

[0069] S1. Raw materials are weighed according to the amounts of the above components to prepare a basic glass batch material. The batch material is melted and kept at 1600°C for 3 hours. After high-temperature homogenization and clarification, a glass liquid is obtained. After the glass liquid is formed by a casting method, it enters an annealing furnace and is kept at 620°C for 2 hours for annealing treatment to obtain a basic glass.

[0070] S2. The base glass is subjected to a nucleation treatment by being kept at 900°C for 0.5h, and then subjected to a crystallization heat treatment by being kept at 1300°C for 0.5h, and then cooled in the furnace to obtain a high-temperature sealed microcrystalline glass, which is then cut, polished, and subjected to subsequent performance tests.

[0071] The main crystalline phase of the high temperature sealing glass-ceramics obtained in this embodiment is Al 0.52 Zr 0.48 O 1.74 (PDF#53-0294) and ZrO 2 (PDF#37-1484), the crystallinity is about 16-19%, and the test results of microcrystalline glass X-ray are as follows Figure 1 As shown; the softening point is 650℃; the thermal expansion coefficient in the temperature range of 20℃-600℃ is 46.3×10 7 ℃ -1 ; Density about 2.445g / cm 3 ; Room temperature resistivity is about 8.00×10 14 Ω·cm; Sealing temperature range 950℃-1025℃.

[0072] Comparative Example 1

[0073] A high-temperature sealing microcrystalline glass, comprising the following components by mass: 50 parts SiO 2 , 16 parts Al 2 O 3 , 14 copies B 2 O 3 , 5 parts ZnO, 5 parts K 2 O, 5 parts CaO, 5 parts TiO 2 ; The sum of the mass percentages of each component is 100%.

[0074] The method for preparing high temperature sealed glass-ceramics comprises the following steps:

[0075] S1. Raw materials are weighed according to the amounts of the above components to prepare a basic glass batch material. The batch material is melted and kept at 1600°C for 3 hours. After high-temperature homogenization and clarification, a glass liquid is obtained. After the glass liquid is formed by a casting method, it enters an annealing furnace and is kept at 620°C for 2 hours for annealing treatment to obtain a basic glass.

[0076] S2. The base glass is subjected to a nucleation treatment by being kept at 900°C for 0.5h, and then subjected to a crystallization heat treatment by being kept at 1300°C for 0.5h, and then cooled in the furnace to obtain a high-temperature sealed microcrystalline glass, which is then cut, polished, and subjected to subsequent performance tests.

[0077] The main crystalline phase of the high temperature sealing glass-ceramics obtained in this comparative example is ZnAl 2 O 4 (PDF#05-0669) and SiO 2 (PDF#52-1425), the crystallinity is about 12-15%, and the test results of the microcrystalline glass X-ray are as follows Figure 3 As shown; the softening point is 693℃; the thermal expansion coefficient in the temperature range of 20℃-600℃ is 46.1×10 7 ℃ -1 ; Density about 2.44g / cm 3 ; Room temperature resistivity is about 1.73×10 13 Ω·cm; Sealing temperature range 900℃-1025℃.

[0078] Comparative Example 2

[0079] A high-temperature sealing microcrystalline glass, comprising the following components by mass: 50 parts SiO 2 , 16 parts Al 2 O 3 , 14 copies B 2 O 3 , 5 parts ZnO, 5 parts K 2 O, 5 parts CaO, 1.4 parts ZrO 2 , 3.6 parts TiO 2 ; The sum of the mass percentages of each component is 100%.

[0080] The method for preparing high temperature sealed glass-ceramics comprises the following steps:

[0081] S1. Raw materials are weighed according to the amounts of the above components to prepare a basic glass batch material. The batch material is melted and kept at 1600°C for 3 hours. After high-temperature homogenization and clarification, a glass liquid is obtained. After the glass liquid is formed by a casting method, it enters an annealing furnace and is kept at 620°C for 2 hours for annealing treatment to obtain a basic glass.

[0082] S2. The base glass is subjected to a nucleation treatment by being kept at 900°C for 0.5h, and then subjected to a crystallization heat treatment by being kept at 1300°C for 0.5h, and then cooled in the furnace to obtain a high-temperature sealed microcrystalline glass, which is then cut, polished, and subjected to subsequent performance tests.

[0083] The main crystalline phase of the high temperature sealing glass-ceramics obtained in this comparative example is ZnAl 2 O 4(PDF#05-0669) and SiO 2 (PDF#52-1425), the crystallinity is about 7-10%, and the test results of microcrystalline glass X-ray are as follows Figure 3 As shown; the softening point is 676℃; the thermal expansion coefficient in the temperature range of 20℃-600℃ is 4.32×10 7 ℃ -1 ; Density about 2.39g / cm 3 ; Room temperature resistivity is about 6.9×10 11 Ω·cm; Sealing temperature range 900℃-1025℃.

[0084] Through reasonable component design, the sealing microcrystalline glass of the present invention has a thermal expansion coefficient similar to that of metals such as Kovar alloy, and has the properties of high softening point, high density, high strength, excellent chemical stability, etc., which improves the sintering strength. At the same time, the preparation method is simple and has broad application prospects.

[0085] The above are only preferred specific implementations of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A high temperature sealing glass-ceramic, It is characterized in that The following components are included in the following mass fractions: 55-65 parts SiO 2 , 8-15 parts Al 2 O 3 10-20 portions B 2 O 3 , 4-10 parts ZnO, 4-10 parts R 2 O, 4-10 parts CaO, 4-10 parts ZrO 2 ; where R 2 O is Na 2 O.K 2 One or more of O; its main crystal phase is Al 0.52 Zr 0.48 O 1.74 and ZrO 2 The crystallinity of the main crystalline phase is 5-19%.

2. A method for preparing the high temperature sealed glass-ceramics as claimed in claim 1, It is characterized in that The following steps are involved: S1. Powdered SiO 2 、Al 2 O 3 , B 2 O 3 、ZnO、R 2 O, CaO, ZrO 2 The mixture is uniformly mixed, melted, homogenized and clarified, and then formed, and then annealed to obtain the basic glass; S2. The base glass is subjected to nucleation and crystallization heat treatments in sequence to obtain the high-temperature sealed microcrystalline glass.

3. The preparation method according to claim 2, It is characterized in that In step S1, the melting temperature is 1500-1600° C., and the melting time is 2-4 hours.

4. The preparation method according to claim 2, It is characterized in that In step S1, the annealing temperature is 580-650° C., and the annealing time is 1-3 hours.

5. The preparation method according to claim 2, It is characterized in that In step S2, the nucleation temperature is 850-950°C, and the nucleation time is 0.5-3h.

6. The preparation method according to claim 2, It is characterized in that In step S2, the crystallization temperature is 1100-1350°C, and the crystallization time is 0.5-3h.

7. Application of high temperature sealing microcrystalline glass obtained by the preparation method as described in any one of claims 2 to 6 in Kovar alloy sealing.

8. The use according to claim 7, It is characterized in that The sealing temperature is 800-1025°C.