A hydrophobic polyester tire base cloth, preparation method and waterproof roll material
By forming a modified corn starch layer on the polyester tire base cloth, the problem of waterproofing performance reduction caused by high water absorption of corn starch is solved, and the waterproof effect and mildew resistance of the asphalt waterproof roll are significantly improved.
Patent Information
- Application Number
- CN202311586898.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-27
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-11-27
AI Technical Summary
The existing polyester tire base cloth in asphalt waterproof rolls has reduced waterproof performance due to the high water absorption of corn starch, and is prone to mold and layering, which affects the waterproofing effect of the rolls.
Using a modified corn starch layer, a hydrophobic polyester tire base cloth is formed by reacting with a hydrophobic modifier and a composition of tetraethyl orthosilicate or hydrophobic silica, reducing water absorption and enhancing mildew resistance, thereby improving waterproof rolls The waterproof effect of the material.
It significantly reduces the water absorption capacity of the polyester tire base cloth, improves the waterproof effect of the waterproof coil, avoids mold and layering caused by water absorption, and improves the quality and waterproof performance of the coil.
Smart Images

Figure BDA0004570134330000111 
Figure BDA0004570134330000121
Abstract
Description
Technical Field
[0001] The invention relates to the field of chemical industry, and in particular to a hydrophobic polyester tire base cloth, a preparation method and a waterproof coiled material. Background Art
[0002] Domestic waterproof membranes with tires, such as asphalt waterproof membranes, mostly use polyester tires as the tire base fabric. Polyester tire base fabric is a non-woven fabric, which is divided into long-fiber polyester tires and short-fiber polyester tires. Long-fiber polyester tires are a new type of tire base fabric used in the preparation of waterproof membranes in recent years. Long-fiber polyester tires use polyester chips as raw materials, and are formed by equipment spinning, needle punching reinforcement, and dipping. Since the polyester tire base fabric has the characteristics of high strength, high elongation and puncture resistance, as well as light weight, high tensile strength, high temperature resistance, freezing resistance, aging resistance, and corrosion resistance, the corresponding waterproof membranes with tires, such as asphalt waterproof membranes, also have corresponding advantages.
[0003] At present, the polyester base cloth used for asphalt waterproofing membrane is usually formed by using corn starch glue. Corn starch can absorb water, and the corresponding waterproofing membrane still has the problem of reduced waterproof performance. Therefore, it is necessary to further improve the traditional polyester base cloth. Summary of the invention
[0004] In view of this, the present invention proposes a hydrophobic polyester base fabric, a preparation method and a waterproof roll. The hydrophobic polyester base fabric has excellent hydrophobicity, oleophilicity and mildew resistance, so that the corresponding waterproof roll has excellent technical indicators and waterproof effect.
[0005] The present invention provides the following technical solutions:
[0006] A hydrophobic polyester tire base fabric comprises a polyester grey fabric and a modified corn starch layer arranged on the surface of the polyester grey fabric.
[0007] The present invention provides the following non-conventional alternatives:
[0008] The hydrophobic polyester tire base fabric comprises 75-90% of the polyester grey cloth and 10-25% of the modified corn starch layer, based on the weight of the hydrophobic polyester tire.
[0009] The modified corn starch used to form the modified corn starch layer is obtained by reacting a composition including corn starch and a hydrophobic modifier.
[0010] The modified corn starch used to form the modified corn starch layer is obtained by reacting a composition including corn starch, a hydrophobic modifier and tetraethyl orthosilicate.
[0011] The modified corn starch used to form the modified corn starch layer is obtained by reacting a composition including corn starch, a hydrophobic modifier and hydrophobic silica.
[0012] The hydrophobic modifier includes one or more of the following components: hexamethyldisilazane, trimethylchlorosilane, and dimethyldichlorosilane.
[0013] The hydrophobic silica comprises one or more of the following components: silica in-situ modified with trimethylchlorosilane, silica in-situ modified with hexamethyldisilazane, and silica in-situ modified with dimethyldichlorosilane.
[0014] The present invention also provides a method for preparing the hydrophobic polyester tire base cloth as described above, which comprises: providing the polyester grey cloth; dip-coating the polyester grey cloth with modified corn starch, and then drying to form the modified corn starch layer and obtain the hydrophobic polyester tire base cloth.
[0015] The present invention also provides a waterproof roll material, which comprises the hydrophobic polyester base fabric as described above.
[0016] Optionally, the waterproof membrane is an asphalt waterproof membrane.
[0017] According to the technical solution of the present invention, the hydrophobic polyester base fabric contains a modified corn starch layer, so that the hydrophobic polyester base fabric has good hydrophobicity and lipophilicity, can effectively reduce the water absorption capacity of the polyester base fabric, and strengthen the adhesion between the hydrophobic polyester base fabric and the waterproof membrane prepreg or coating material such as asphalt prepreg; furthermore, the hydrophobic polyester base fabric has good mildew resistance, can effectively improve the delamination of the waterproof membrane caused by mildew of the base fabric, and improve the waterproof effect of the waterproof membrane. DETAILED DESCRIPTION
[0018] For ease of understanding of the present invention, the present invention will be described more fully below with reference to examples. Preferred embodiments of the present invention are provided in the examples. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0019] At present, the polyester base fabric used in asphalt waterproofing rolls is formed using corn starch glue, but corn starch has high water absorption, which leads to the corresponding asphalt waterproofing rolls generally having an unqualified mass increase percentage after immersion in water, and the starch after absorbing water is prone to mildew, and the polyester base fabric will be delaminated, which reduces the waterproof effect of the roll, and further causes water seepage in the building. In this regard, the hydrophobic polyester base fabric in the embodiment of the present invention can significantly reduce the water absorption of the base fabric in the asphalt waterproofing roll when used for waterproofing rolls, thereby ensuring that the mass increase value of the waterproofing roll after immersion in water meets the relevant standards, and can also improve the mildew and even delamination of the waterproofing roll caused by the base fabric absorbing water, thereby preventing leakage in the building; and the oil absorption performance of the hydrophobic polyester base fabric enhances the bonding between the polyester base fabric and the prepreg used to prepare the waterproofing roll, achieving better bonding between the polyester base fabric and the prepreg, and further improving the delamination of the waterproofing roll.
[0020] The hydrophobic polyester tire base fabric in the embodiment of the present invention comprises a polyester grey fabric and a modified corn starch layer arranged on the surface of the polyester grey fabric. The hydrophobic polyester tire base fabric comprises 75-90%, for example 75-85%, of the polyester grey fabric and 10-25%, for example 15-25% of the modified corn starch layer. Based on the weight of the hydrophobic polyester tire, the sum of the weights of the components in the hydrophobic polyester tire base fabric is 100%. The thickness of the hydrophobic polyester tire base fabric is 1.0-1.5 mm, for example 1.1-1.3 mm. Thus, while ensuring the tensile strength of the polyester tire base fabric, the polyester tire base fabric has improved hydrophobicity and mildew resistance.
[0021] Polyester grey cloth is a polyester fiber non-woven fabric, and the polyester fiber is usually polyester fiber, that is, polyethylene terephthalate (PET). The polyester grey cloth can be a commercially available product or prepared by a method known to those skilled in the art, for example, by spinning and weaving polyester chips using a spunbond method. Specifically, the polyester chips are melted and extruded at high temperature, and after passing through a spinneret, they are driven by a high-speed airflow and instantly cooled to form filaments. The filaments are evenly swung to a web laying machine through a swinging wire plate according to the direction in which they are set. The web laying machine drives the flattened fiber web to form a polyester grey cloth through a pre-needling and acupuncture process. The polyester chips are usually fiber-grade polyester chips, and their intrinsic viscosity is 0.5-0.9dl / g, melting point is 240-280℃, and carbon dioxide content is 0.1-0.5%; determined according to GB / T14190-2017.
[0022] The modified corn starch layer is formed by dip-coating the modified corn starch on the polyester grey cloth. The modified corn starch is obtained by reacting a composition comprising corn starch and a hydrophobic modifier. Furthermore, the modified corn starch is obtained by reacting a composition comprising corn starch, a hydrophobic modifier and optionally tetraethyl orthosilicate. Without being bound by any theory, the inventors believe that the hydrophobic modifier can not only modify the silica generated by tetraethyl orthosilicate, but also modify the corn starch, so that the modified corn starch is easier to combine with the generated hydrophobic silica, so that a more hydrophobic modified corn starch can be prepared. Similarly, the hydrophobic modifier can also directly modify the corn starch to obtain a modified corn starch. The hydrophobic modifier may include one or more of the following components: hexamethyldisilazane, trimethylchlorosilane, dimethyldichlorosilane; for example, hexamethyldisilazane or trimethylchlorosilane, such as hexamethyldisilazane.
[0023] Specifically, the modified corn starch is obtained by reacting a composition comprising the following components: 10-25% corn starch, 10-30% such as 14-29.5% hydrophobic modifier, 0-5% such as 0-3.5% tetraethyl orthosilicate, 25-35% ethanol, 20-50% water, 0.1-0.6% hydrolyzing agent, 0.1-0.6% ammonia water and 14-20% such as 17-18.5% solvent, based on the weight of the composition; the sum of the weight percentages of the components in the composition is 100%.
[0024] In an embodiment of the present invention, modified corn starch is prepared by the following steps:
[0025] 1) mixing corn starch and ethanol for 0.4-0.6 hours and drying to obtain substance A;
[0026] II) mixing substance A with water and a hydrolyzing agent in sequence to obtain substance B;
[0027] III) mixing substance B with a solvent and a hydrophobic modifier to obtain substance C;
[0028] IV) Optionally add tetraethyl orthosilicate to substance C, mix, then add ammonia water to obtain a gel.
[0029] V) dispersing the obtained gel in ethanol to obtain modified corn starch.
[0030] Step I) comprises mixing corn starch with ethanol, such as anhydrous ethanol, at 70-90° C. under magnetic stirring at 100-300 r / min for 0.4-0.6 hours, and drying to obtain defatted corn starch of substance A. Step II) comprises mixing substance A with water, cooling and refluxing, stirring and mixing at a speed of 500-700 r / min, raising the temperature to 70-90° C., and maintaining it for 0.5-2 hours; then lowering the temperature to 40-60° C., adding a hydrolyzing agent to the mixture until the pH is adjusted to 2-4, and stirring at a speed of 500-700 r / min for 2-6 hours to obtain substance B. The hydrolyzing agent is used to hydrolyze the hydrophobic modifier and tetraethyl orthosilicate so as to react with corn starch later; it can generally include one or more of the following components: oxalic acid, hydrochloric acid, acetic acid, sulfuric acid, such as oxalic acid or hydrochloric acid, such as oxalic acid. In step III), the mixture is stirred at a speed of 100-300 r / min for 0.5-1.5 hours. The solvent may be an organic solvent known to those skilled in the art, for example, it may include one or more of the following components: N,N-dimethylformamide, n-hexane, ethanol; for example, it may be N,N-dimethylformamide or ethanol.
[0031] In step IV), after the addition of tetraethyl orthosilicate is completed, stir at a speed of 500-700r / min at 35-60°C for 1-3 hours, then add ammonia water until the pH is adjusted to 8-10, and then stand at the same temperature for 20-28 hours to obtain a gel. The hydrophobic modifier can modify the surface of the corn starch so that the modified corn starch is more easily combined with the generated silica. In addition, the hydrophobic modifier and tetraethyl orthosilicate can be added at the same time. In certain embodiments of the present invention, tetraethyl orthosilicate may not be added in step IV), and modified corn starch can also be obtained. In step V), the gel is ultrasonically dispersed in ethanol to obtain modified corn starch directly used for dip-coating polyester grey cloth.
[0032] The modified corn starch for forming the modified corn starch layer in the embodiment of the present invention can also be obtained by reacting a composition comprising corn starch, a hydrophobic modifier, and hydrophobic silica. Specifically, the modified corn starch can be obtained by modifying the corn starch with a hydrophobic modifier and then modifying it with hydrophobic silica. Alternatively, the modified corn starch is also obtained by reacting a composition comprising hydrophobic corn starch and hydrophobic silica. Specifically, the modified corn starch can be obtained by directly modifying the hydrophobic corn starch with hydrophobic silica. The use of pyridine, a carcinogen, is avoided during the preparation of the modified corn starch, which is safe and environmentally friendly.
[0033] The hydrophobic silica may be a commercially available product or may be prepared by a method well known to those skilled in the art, such as a sol-gel method; its specific surface area is 100-300 m 2 / g, the silica content is not less than 99.5%, based on the weight of the hydrophobic silica. Commonly used hydrophobic silicas include trimethylchlorosilane in-situ modified silica, hexamethyldisilazane in-situ modified silica or dimethyldichlorosilane in-situ modified silica; for example, R974 or R972 purchased from Evonik Degussa.
[0034] The hydrophobic corn starch can be a commercially available product or can be prepared by methods well known to those skilled in the art. For example, the hydrophobic corn starch is usually prepared by modifying corn starch with a hydrophobic modifier, and the hydrophobic modifier has the definition as described above.
[0035] The contact angle (also called hydrophobicity) of the hydrophobic polyester tire base fabric with water at 25°C may be greater than 100°, as determined by the contact angle measurement method of GB / T24368-2009. The percentage increase in mass of the hydrophobic polyester tire base fabric after immersion in water is less than 10%, based on the weight of the modified corn starch, as determined by the polyester tire base fabric test directly without applying asphalt rubber in accordance with Section 6.12 of GB18242-2008. The oil absorption of the hydrophobic polyester tire base fabric is greater than 40 ml / 100 g, as determined in accordance with Part 15 of GB / T5211.15-2014; the total colony count of the hydrophobic polyester tire base fabric is less than 200 CFU / G, for example, less than 160 CFU / G, as determined in accordance with GB / T8885-2008.
[0036] The hydrophobic polyester tire base fabric is obtained by dipping the polyester grey fabric with modified corn starch and then drying it. The dipping requires that the modified corn starch fully soaks the polyester grey fabric, and is usually dipped for 0.3-1min at room temperature. Drying is usually carried out in a drying oven at a temperature of 180-200°C until the moisture content in the tire base fabric reaches ≤0.5%, based on the weight of the tire base fabric. After drying, the hydrophobic polyester tire base fabric can be cut into a width of about 1m and rolled up for storage.
[0037] Therefore, an embodiment of the present invention also provides a method for preparing the hydrophobic polyester tire base fabric, which includes providing a polyester grey cloth, which can be a commercially available product or prepared by a method known to those skilled in the art, such as spinning and molding polyester chips to obtain a polyester grey cloth, and the weight of the polyester grey cloth is 150-170 g / m 2 The polyester fabric is dipped with modified corn starch and then dried to form a modified corn starch layer to obtain a hydrophobic polyester tire base fabric; the weight of the hydrophobic polyester tire base fabric is 190-210g / m 2 .
[0038] The waterproofing membrane in the embodiment of the present invention comprises the hydrophobic polyester base fabric as described above. The waterproofing membrane is an asphalt waterproofing membrane, such as various modified asphalt waterproofing membranes, such as elastomeric asphalt waterproofing membrane (SBS modified) and plastomer asphalt waterproofing membrane (APP modified). The preparation method of the waterproofing membrane is well known to those skilled in the art, for example, usually at a temperature of 165-190° C., such as 165-180° C., at normal pressure, a prepreg such as an asphalt material for preparing the waterproofing membrane is impregnated on the above-mentioned hydrophobic polyester base fabric, and then an asphalt coating material is coated on at least one side thereof to form a coating layer, and optionally then covered with an isolation film to obtain the waterproofing membrane.
[0039] The present invention is described below by specific examples. The examples described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention. If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in this area or the product instructions are used. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be obtained commercially.
[0040] raw material:
[0041] Corn starch: food grade, purchased from Jinan Huayi Chemical Technology Co., Ltd.
[0042] Hexamethyldisilazane, trimethylchlorosilane, tetraethyl orthosilicate, anhydrous ethanol and N,N-dimethylformamide were all of analytical grade and purchased from Aladdin Reagents.
[0043] Oxalic acid was of analytical grade and purchased from Xilong Science.
[0044] Polyester chips: fiber grade, intrinsic viscosity 0.71 dl / g; semi-matt chips; purchased from Hubei Lvyu Environmental Protection Co., Ltd.
[0045] Hydrophobic silica: surface area 200m 2 / g, modified with dimethyldichlorosilane, trade name R974, purchased from Evonik Degussa.
[0046] 1. Preparation of polyester tire base cloth
[0047] Example 1
[0048] (1) Preparation of modified corn starch
[0049] I) weighing 273 g corn starch into a 1000 ml three-necked flask, adding 500 g anhydrous ethanol, defatting for half an hour under magnetic stirring at a speed of 150 r / min at 80° C., and then drying in a drying oven at a temperature of 50° C. for 2 hours to obtain substance A defatted corn starch;
[0050] II) Add all of substance A into a 1000ml three-necked flask, measure 500g of deionized water, pour it into substance A, raise the water temperature to 80°C, reflux and stir at 600r / min for 1h; then cool down to 50°C under reflux, add 5g of oxalic acid with a dropper, and after the addition, reflux at 50°C and stir at 600r / min for 4h to obtain substance B;
[0051] III) Add 200 g of N,N-dimethylformamide and 161 g of hexamethyldisilazane into another 1000 ml beaker, and stir and disperse at a speed of 150 r / min for half an hour to obtain substance C;
[0052] IV) taking half of the substance B obtained in step II, pouring it into the substance C, and then adding 40 g of tetraethyl orthosilicate, and after the addition, stirring and reacting at 50° C. and 600 r / min for 2 h, and then adding 2.5 g of ammonia water to the obtained mixture until the pH of the mixture is 9; and then standing and reacting at 50° C. for 24 h to obtain a gel;
[0053] V) weighing the obtained gel, and ultrasonically dispersing it with 100 g of anhydrous ethanol to obtain hydrophobic corn starch.
[0054] The composition and related properties of the obtained modified corn starch are shown in Table 1.
[0055] (2) Preparation of polyester grey cloth
[0056] The polyester chips were melt extruded at 290°C in an extruder (model JHM420-20-I, purchased from JHM Machinery Group Co., Ltd.), passed through a 48-hole spinneret, and driven by an air flow at a rate of 2000 m / min, and instantly cooled to form filaments with a diameter of 20 μm. The filaments were evenly swung to a 6.8-meter web laying machine according to the set direction through a swinging wire plate. The web laying machine drove the flat fiber web to undergo pre-needling and needling processes to form a 160 g / m 2 Polyester grey cloth.
[0057] (3) Preparation of hydrophobic polyester tire base fabric
[0058] 160g of one square meter of the polyester fabric was dipped in the modified corn starch prepared above (the amount was such that the polyester fabric was immersed) for 30 seconds; then it was sent to a drying oven and dried at 190°C for 2 hours until the moisture content reached ≤0.5%, and 200g / m 2 Hydrophobic polyester tire base fabric 1.
[0059] Embodiment 2-6
[0060] The steps of Example 1 were repeated, except that (1) the composition of the raw materials in the preparation of the modified corn starch was changed, and (3) the ratio of the polyester grey cloth to the corn starch layer in the preparation of the polyester tire base cloth was changed.
[0061] The composition and related properties of modified corn starch are shown in Table 1.
[0062] Example 7: Modification with hexamethyldisilazane and then with finished hydrophobic silica
[0063] The steps described in Example 1 were repeated, except that: (1) the preparation of modified corn starch included
[0064] I) weighing 273 g corn starch into a 1000 ml three-necked flask, adding 500 g anhydrous ethanol, defatting for half an hour under magnetic stirring at a speed of 150 r / min at 80° C., and then drying in a drying oven at a temperature of 50° C. for 2 hours to obtain substance A defatted corn starch;
[0065] II) Add all of substance A into a 1000ml three-necked flask, measure 500g of deionized water, pour it into substance A, raise the water temperature to 80°C, reflux and stir at 600r / min for 1h; then cool down to 50°C under reflux, add 5g of oxalic acid with a dropper, and after the addition, reflux at 50°C and stir at 600r / min for 4h to obtain substance B;
[0066] III) Add 200 g of N,N-dimethylformamide and 161 g of hexamethyldisilazane into another 1000 ml beaker, and stir and disperse at a speed of 150 r / min for half an hour to obtain substance C;
[0067] IV) taking half of the substance B obtained in step II, pouring it into the substance C, and then adding 8 g of hydrophobic silica, after the addition is completed, stirring and reacting at 50° C. and 600 r / min for 2 h, and then adding 2.5 g of ammonia water to the obtained mixture until the pH of the mixture is 9; and then standing and reacting at 50° C. for 24 h to obtain a gel;
[0068] V) weighing the obtained gel, and dispersing it ultrasonically with 100 g of anhydrous ethanol to obtain hydrophobic corn starch.
[0069] The composition and related properties of modified corn starch are shown in Table 1.
[0070] Example 8
[0071] The steps of Example 7 were repeated, except that in the preparation of (1) modified corn starch, the amount of hydrophobic silicon dioxide added in step IV) was 4 g.
[0072] The composition and related properties of modified corn starch are shown in Table 1.
[0073] Example 9
[0074] The procedure of Example 1 was repeated except that in step III) of (1) preparation of modified corn starch, hexamethyldisilazane was replaced with trimethylchlorosilane.
[0075] Comparative Example 1: Directly use ordinary corn starch
[0076] (1) Preparation of corn starch paste
[0077] 273 g of corn starch was mixed with 500 g of water at 80° C. and stirred at 150 r / min for gelatinization to obtain corn starch paste. The composition and related properties of the corn starch paste are shown in Table 1.
[0078] (2) Preparation of polyester grey cloth
[0079] The steps of Example 1 were repeated.
[0080] (3) Preparation of polyester tire base fabric
[0081] The steps of Example 1 were repeated.
[0082] Table 1 Composition and properties of polyester tire base fabrics of various embodiments and comparative examples
[0083]
[0084]
[0085] As can be seen from Table 1, the hydrophobicity, oil absorption and total bacterial count of the hydrophobic polyester tire base cloth provided by the present invention are better than those of the polyester tire base cloth prepared using ordinary corn starch.
[0086] 2. Application Examples
[0087] The prepreg was impregnated on the polyester tire base fabric prepared in the above-mentioned embodiments and comparative examples at a temperature of 165±5°C under normal pressure; then it was immersed in a coating material pool containing a coating material for 1 minute to obtain a composite; then the surfaces of both sides of the obtained composite were covered with a PE isolation film, and a 3mm thick asphalt waterproofing membrane conforming to GB 18242-2008I type was prepared by double-roll extrusion molding; wherein the thickness of the lower surface coating layer was 1.0mm, the thickness of the polyester tire base fabric was 1.1mm, and the weight of the prepreg was 0.6kg / m 2 .
[0088] The prepreg includes 90 wt % of 90# asphalt and 10 wt % of 10# asphalt.
[0089] The coating material comprises 45 wt% of 90# asphalt, 5 wt% of 61# base oil, 5 wt% of SBS modifier, 3 wt% of SIS modifier, 2 wt% of SBR modifier, 20 wt% of rubber powder and 20 wt% of stone powder.
[0090] According to GB 18242-2008, various properties of the obtained asphalt waterproof membrane were tested, and the results are shown in Table 2.
[0091] Table 2 Performance of asphalt waterproofing membranes corresponding to various embodiments and comparative examples
[0092]
[0093] Compared with the waterproof roll using ordinary corn starch, the waterproof roll in the embodiment of the present invention significantly reduces the mass increase value after immersion in water while ensuring the tensile force and elongation. For example, the mass increase value of the waterproof roll prepared in Example 1 after immersion in water is only 0.2%, which is one quarter of the waterproof roll prepared in Comparative Example 1.
[0094] The above specific implementations do not constitute a limitation on the protection scope of the present invention. It should be understood by those skilled in the art that various modifications, combinations, sub-combinations and substitutions may occur depending on design requirements and other factors. Any modification, equivalent substitution and improvement made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A hydrophobic polyester tire base fabric, characterized in that: It includes a polyester grey cloth and a modified corn starch layer arranged on the surface of the polyester grey cloth; The modified corn starch used to form the modified corn starch layer is prepared by the following steps: I) mixing corn starch and ethanol for 0.4-0.6 hours and drying to obtain substance A; II) mixing substance A with water and a hydrolyzing agent in sequence to obtain substance B; III) mixing substance B with a solvent and a hydrophobic modifier to obtain substance C; IV) adding tetraethyl orthosilicate or hydrophobic silica to substance C, mixing, and then adding ammonia water to obtain a gel; V) dispersing the obtained gel in ethanol to obtain modified corn starch; The hydrophobic modifier comprises one or more of the following components: hexamethyldisilazane, trimethylchlorosilane, and dimethyldichlorosilane.
2. The hydrophobic polyester tire base fabric according to claim 1, characterized in that: The hydrophobic polyester tire base fabric comprises 75-90% of the polyester grey cloth and 10-25% of the modified corn starch layer, based on the weight of the hydrophobic polyester tire.
3. The hydrophobic polyester tire base fabric according to claim 1, characterized in that: The hydrophobic silica comprises one or more of the following components: silica in-situ modified with trimethylchlorosilane, silica in-situ modified with hexamethyldisilazane, and silica in-situ modified with dimethyldichlorosilane.
4. A method for preparing the hydrophobic polyester tire base fabric according to claim 1, characterized in that: include: Providing the polyester grey cloth; The polyester grey cloth is dip-coated with modified corn starch and then dried to form the modified corn starch layer and obtain the hydrophobic polyester tire base cloth.
5. A waterproof roll material, characterized in that: It comprises the hydrophobic polyester tire base fabric according to any one of claims 1 to 3.