A lithium battery diaphragm coating composition and preparation method thereof

The heat resistance and electrolyte of the separator material are solved by using a composition of polyimide, modified gel and deionized water on the lithium-ion battery separator. Adsorption problem improves the cycle stability and charge and discharge capacity of the battery.

CN117625036BActive Publication Date: 2024-11-12FOSHAN DAWEI TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410100710.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-25
Publication Date
2024-11-12
Estimated Expiration
2044-01-25

AI Technical Summary

Technical Problem

The existing lithium-ion battery separator materials have poor heat resistance and low adsorption efficiency for electrolyte, making it difficult to meet the requirements of high-end market for large current and high-rate discharge.

Method used

Using a lithium battery separator coating composition, including polyimide, modified gel and deionized water, the separator is formed by preparing modified graphene oxide and carboxylated cellulose aerogel to form a porous amorphous material and improve the separator. heat shrinkage resistance and electrochemical properties.

Benefits of technology

Improve the heat resistance and electrochemical performance of the membrane, enhance the adsorption capacity and liquid retention rate of the electrolyte, reduce the interface energy between graphene oxide and surface polymer, promote electron transport and charge transport, and improve lithium ions Cycling stability and fast charging and discharging capabilities of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention discloses a lithium battery diaphragm coating composition and a preparation method thereof, and relates to the technical field of lithium ion batteries. The lithium battery diaphragm coating composition of the present invention comprises the following raw materials in weight percentage: polyimide 15-35wt%, modified gel 20-40wt%, deionized water 25-65wt%, and the sum of each raw material component is 100%; wherein the modified gel comprises graphene oxide and carboxylated cellulose aerogel of which p-phenylenediamine and aniline are polymerized in situ on the surface. The modified gel prepared in the present application is added to the coating composition to effectively improve the porosity, water absorption and water retention of the coating; the coating is applied to the surface of the diaphragm to give the material high ionic conductivity and electrochemical stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a lithium battery diaphragm coating composition and a preparation method thereof. Background Art

[0002] With the widespread use of electronic devices such as electric vehicles, mobile phones, and laptops, lithium-ion batteries have become one of the most commonly used rechargeable batteries. As an indispensable component of lithium-ion batteries, the separator plays many important roles, such as isolating the electrolyte, preventing direct short circuits between the positive and negative electrodes, and maintaining ion conductivity. Therefore, improving the performance and stability of lithium-ion battery separators is of great significance to improving the performance and safety of lithium-ion batteries.

[0003] At present, most lithium-ion battery separators are made of polyolefin materials. Polyolefin materials are hydrophobic in structure and have low porosity in morphology, which leads to poor electrochemical performance of lithium-ion batteries. In terms of process, polyolefin separators are oriented by stretching, and the molecular chains are deoriented at high temperatures, resulting in uneven shrinkage. In addition, the poor heat resistance of the material itself affects the high-temperature safety of lithium-ion batteries. Generally, it is difficult to meet the requirements of high-end market applications of lithium-ion batteries for high current and high-rate discharge, high heat resistance and dimensional stability, and good ability to absorb and retain electrolytes. In order to improve the above problems, the surface of polyolefin separators is often modified by coating technology. Summary of the invention

[0004] The purpose of the present invention is to provide a lithium battery separator coating composition and a preparation method thereof, so as to solve the following technical problems:

[0005] The existing diaphragm material is a microporous polyolefin material, which has poor heat resistance and low efficiency in adsorbing and retaining electrolyte.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A lithium battery separator coating composition, comprising the following raw materials in percentage by weight: 15-35wt% of polyimide, 20-40wt% of modified gel, and 25-65wt% of deionized water, the sum of the raw material components being 100%;

[0008] The preparation method of the modified gel comprises the following steps:

[0009] S1: Add graphene oxide and deionized water into a reaction bottle, disperse them evenly, add p-phenylenediamine, control the temperature to 60-70°C, keep warm for 3-6 hours under stirring conditions, centrifuge, wash, and dry to obtain component 1;

[0010] S2: Add aniline and hydrochloric acid solution into the reaction kettle, disperse evenly, add component 1, disperse evenly, add ammonium persulfate, control the temperature at 0-10°C, keep warm for 6-9h, wash and dry to obtain modified graphene oxide;

[0011] S3: Add modified graphene oxide, carboxylated cellulose aerogel and deionized water into a reactor, disperse them evenly, control the temperature at 0-5°C, and perform ultrasonic dispersion for 0.5-1h to obtain a modified gel.

[0012] As a further embodiment of the present invention: the preparation method of graphene oxide comprises the following steps:

[0013] B1: Add 10g graphite powder, 8.3g potassium persulfate, 8.3g phosphorus pentoxide into a reaction bottle, 40mL concentrated sulfuric acid, control the temperature at 70-80℃, and keep warm for 6-12h; add 660mL deionized water and let stand for 24h, wash with water until neutral, and dry to obtain pre-oxidized graphite powder;

[0014] B2: 10g pre-oxidized graphite powder and 360mL concentrated sulfuric acid were added to the reaction bottle, the temperature was controlled at 0-5℃, 45g potassium permanganate was added under stirring, the mixture was kept warm for 1-3h under stirring, the temperature was controlled at 20-30℃, the mixture was kept warm for 1-3h under stirring, 400mL distilled water was added, the temperature was controlled at 30-40℃, 1500mL distilled water was added, the mixture was evenly dispersed, 300mL 30wt% H2O2 was added to terminate the reaction, and the mixture was washed with water until neutral to obtain graphene oxide.

[0015] As a further solution of the present invention: in S1, the addition ratio of graphene oxide, deionized water and p-phenylenediamine is 4 g: 4-40 mL: 1-3 g.

[0016] As a further embodiment of the present invention: the hydrochloric acid solution in S2 is a 1-1.5 mol / L hydrochloric acid aqueous solution; the addition ratio of aniline, hydrochloric acid solution, component one, and ammonium persulfate is 5 g: 10-12.5 mL: 1-2 g: 1-6 g.

[0017] As a further solution of the present invention: in S3, the modified graphene oxide, carboxylated cellulose aerogel, and deionized water are added in a ratio of 0.3-0.5 g: 1 g: 50-100 mL.

[0018] As a further embodiment of the present invention: the preparation method of carboxylated cellulose aerogel comprises the following steps:

[0019] A1: Add sodium hydroxide, urea, deionized water and potassium chloride into a reaction bottle and disperse them evenly, control the temperature at -10 to 0°C, add cellulose powder, disperse them evenly, centrifuge, let stand, and vacuum freeze-dry to obtain cellulose aerogel;

[0020] A2: Add cellulose aerogel and deionized water into a reaction bottle, disperse them evenly, add TEMPO and sodium bromide, disperse them evenly, adjust the pH to 9-11, add NaClO solution, maintain the pH to 9-11 during the reaction, add anhydrous ethanol to terminate the reaction, wash with water, and dry to obtain carboxylated cellulose aerogel.

[0021] As a further solution of the present invention: the specific steps of vacuum freeze-drying in A1 are as follows: cold trap temperature -60°C, vacuum degree -0.1 MPa, and freeze-drying for 48 hours.

[0022] As a further solution of the present invention: in A1, the addition ratio of sodium hydroxide, urea, deionized water, potassium chloride and cellulose powder is 5-10 g: 10-20 g: 70-150 mL: 2-5 g: 5 g.

[0023] As a further embodiment of the present invention: the NaClO solution in A2 is a 5-10wt% NaClO aqueous solution; the addition ratio of cellulose aerogel, deionized water, TEMPO, sodium bromide, and NaClO solution is 10g: 100-200mL: 0.02-0.05g: 15-30g: 20-30mL.

[0024] A method for preparing any of the above-mentioned lithium battery separator coating compositions comprises the following steps: dissolving polyimide in deionized water, dispersing the polyimide uniformly, adding modified gel, dispersing the polyimide uniformly, and obtaining the lithium battery separator coating composition.

[0025] Beneficial effects of the present invention:

[0026] The present application uses unmodified cellulose as a raw material, and adds a small amount of inorganic salt to a sodium hydroxide-urea aqueous solution to induce and promote the system to form a gel. The aerogel prepared in the present application is a porous amorphous material composed of polymer molecules that are mutually aggregated to form a network skeleton, and has the characteristics of low density and high porosity; and TEMPO (2,2,6,6-tetramethylpiperidinyl oxide) is used to react with the hydroxymethyl in cellulose to obtain TEMPO-oxidized cellulose with a high degree of oxidation, so that the surface of the cellulose aerogel is carboxylated to obtain a carboxylated cellulose aerogel; TEMPO oxidation treatment increases the permeability of the aerogel surface. Graphene oxide is then used as a raw material to perform amination with p-phenylenediamine to obtain component one; aniline is used to perform in-situ polymerization on the surface of graphene oxide to obtain graphene oxide with a conductive polymer coated on the surface; finally, the modified graphene oxide and carboxylated cellulose aerogel are used as raw materials to form an ionic bond between -NH- on the modified graphene oxide and -COOH of the carboxylated cellulose aerogel to obtain a modified gel; the prepared modified gel is added to a coating, and the coating is applied to the surface of a diaphragm to give the diaphragm a porous structure; the modified gel is tightly connected and stacked by an organic adhesive to improve the heat shrinkage resistance of the diaphragm and effectively prevent heat shrinkage.

[0027] The -C= of the modified graphene oxide prepared in this application forms a π-π conjugated structure with the -NH- of the polymer on the surface, which is conducive to the transfer of electrons, significantly reduces the interfacial energy between graphene oxide and the surface polymer, and effectively improves the capacitance and cycle stability of the material; the coating prepared in this application gives the material high conductivity to promote the rapid transmission of charge and improve the rapid charge and discharge capacity of the material. The rich -OH, -COOH-, -NH2 and other functional groups in the modified gel prepared in this application have good affinity with the electrolyte. At the same time, the porous fibrous structure of the modified gel increases the porosity of the diaphragm, which is conducive to the adsorption of the electrolyte by the material, and as time increases, it still maintains a good liquid retention rate. It can be seen that the coating does have a good affinity for the electrolyte. The coating prepared in this application is coated on the surface of the diaphragm, and the interface impedance between the diaphragm and the electrode is greatly reduced, which is conducive to the cycle stability of the lithium-ion battery. DETAILED DESCRIPTION

[0028] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1

[0029] The preparation method of graphene oxide comprises the following steps:

[0030] B1: Add 10g graphite powder, 8.3g potassium persulfate, 8.3g phosphorus pentoxide into a reaction bottle, 40mL concentrated sulfuric acid, control the temperature at 70-80℃, and keep warm for 6-12h; add 660mL deionized water and let stand for 24h, wash with water until neutral, and dry to obtain pre-oxidized graphite powder;

[0031] B2: 10g pre-oxidized graphite powder and 360mL concentrated sulfuric acid were added to the reaction bottle, the temperature was controlled at 0℃, 45g potassium permanganate was added under stirring, the mixture was kept warm for 1h under stirring, the temperature was then controlled at 20℃, the mixture was kept warm for 3h under stirring, 400mL distilled water was added, the temperature was controlled at 40℃, 1500mL distilled water was added, the mixture was evenly dispersed, 300mL 30wt% H2O2 was added to terminate the reaction, and the mixture was washed with water until neutral to obtain graphene oxide. Example 2

[0032] The preparation method of carboxylated cellulose aerogel comprises the following steps:

[0033] A1: 10 g of sodium hydroxide, 20 g of urea, 140 mL of deionized water, and 4 g of potassium chloride were added to a reaction bottle and dispersed evenly. The temperature was controlled at 0°C, 10 g of cellulose powder was added, dispersed evenly, centrifuged, allowed to stand, and freeze-dried for 48 h under the conditions of a cold trap temperature of -60°C and a vacuum degree of -0.1 MPa to obtain cellulose aerogel;

[0034] A2: 10 g of cellulose aerogel and 100 mL of deionized water were added to a reaction bottle and dispersed evenly. 0.02 g of TEMPO and 15 g of sodium bromide were added and dispersed evenly. The pH was adjusted to 9 with a 0.1 mol / L NaOH aqueous solution. 20 mL of NaClO solution was added. During the reaction, 0.1 mol / L NaOH aqueous solution was added to maintain the pH at 9. Anhydrous ethanol was added to terminate the reaction. The mixture was washed with water and dried to obtain carboxylated cellulose aerogel. Example 3

[0035] The preparation method of carboxylated cellulose aerogel comprises the following steps:

[0036] A1: Add 20g sodium hydroxide, 40g urea, 300mL deionized water and 10g potassium chloride into a reaction bottle and disperse them evenly. Control the temperature at -10°C, add 10g cellulose powder, disperse them evenly, centrifuge, let stand, freeze-dry for 48h under the conditions of cold trap temperature of -60°C and vacuum degree of -0.1MPa, freeze-dry for 48h to obtain cellulose aerogel;

[0037] A2: Add 10g cellulose aerogel and 200mL deionized water into a reaction bottle and disperse them evenly. Add 0.05g TEMPO and 30g sodium bromide and disperse them evenly. Adjust the pH to 11 with 0.1mol / L NaOH aqueous solution. Add 30mL NaClO solution. During the reaction, add 0.1mol / L NaOH aqueous solution to maintain the pH at 11. Add anhydrous ethanol to terminate the reaction. Wash with water and dry to obtain carboxylated cellulose aerogel. Example 4

[0038] The preparation method of the modified gel comprises the following steps:

[0039] S1: 40 g of graphene oxide prepared in Example 1 and 40 mL of deionized water were added to a reaction bottle, dispersed evenly, 10 g of p-phenylenediamine was added, the temperature was controlled at 60° C., the mixture was kept warm for 3 h under stirring, centrifuged, washed, and dried to obtain component 1;

[0040] S2: Add 40g aniline and 80mL 1mol / L hydrochloric acid aqueous solution into the reactor, disperse evenly, add 8g component 1, disperse evenly, add 8g ammonium persulfate, control the temperature to 0°C, keep warm for 6h, wash and dry to obtain modified graphene oxide;

[0041] S3: 25 g of modified graphene oxide, 50 g of the carboxylated cellulose aerogel prepared in Example 2, and 2500 mL of deionized water were added into a reactor, dispersed evenly, the temperature was controlled at 0° C., and ultrasonic dispersion was performed for 0.5 h to obtain a modified gel. Example 5

[0042] The preparation method of the modified gel comprises the following steps:

[0043] S1: 40 g of graphene oxide prepared in Example 1 and 400 mL of deionized water were added to a reaction bottle, dispersed evenly, 30 g of p-phenylenediamine was added, the temperature was controlled to 70° C., the mixture was kept warm for 6 h under stirring, centrifuged, washed, and dried to obtain component 1;

[0044] S2: Add 40g of aniline and 100mL of 1.5mol / L hydrochloric acid aqueous solution into the reactor, disperse evenly, add 16g of component 1, disperse evenly, add 48g of ammonium persulfate, control the temperature at 10°C, keep warm for 9h, wash and dry to obtain modified graphene oxide;

[0045] S3: 25 g of modified graphene oxide, 50 g of the carboxylated cellulose aerogel prepared in Example 2, and 2500 mL of deionized water were added into a reactor, dispersed evenly, the temperature was controlled at 5° C., and ultrasonic dispersion was performed for 1 h to obtain a modified gel. Example 6

[0046] The preparation method of the modified gel comprises the following steps:

[0047] S1: 40 g of graphene oxide prepared in Example 1 and 40 mL of deionized water were added to a reaction bottle, dispersed evenly, 10 g of p-phenylenediamine was added, the temperature was controlled at 60° C., the mixture was kept warm for 3 h under stirring, centrifuged, washed, and dried to obtain component 1;

[0048] S2: Add 40g aniline and 80mL 1mol / L hydrochloric acid aqueous solution into the reactor, disperse evenly, add 8g component 1, disperse evenly, add 8g ammonium persulfate, control the temperature to 0°C, keep warm for 6h, wash and dry to obtain modified graphene oxide;

[0049] S3: 25 g of modified graphene oxide, 50 g of the carboxylated cellulose aerogel prepared in Example 3, and 2500 L of deionized water were added into a reactor, dispersed evenly, the temperature was controlled at 0° C., and ultrasonic dispersion was performed for 0.5 h to obtain a modified gel. Example 7

[0050] The preparation method of the modified gel comprises the following steps:

[0051] S1: 40 g of graphene oxide prepared in Example 1 and 400 mL of deionized water were added to a reaction bottle, dispersed evenly, 30 g of p-phenylenediamine was added, the temperature was controlled to 70° C., the mixture was kept warm for 6 h under stirring, centrifuged, washed, and dried to obtain component 1;

[0052] S2: Add 40g of aniline and 100mL of 1.5mol / L hydrochloric acid aqueous solution into the reactor, disperse evenly, add 16g of component 1, disperse evenly, add 48g of ammonium persulfate, control the temperature at 10°C, keep warm for 9h, wash and dry to obtain modified graphene oxide;

[0053] S3: 25 g of modified graphene oxide, 50 g of the carboxylated cellulose aerogel prepared in Example 3, and 2500-5000 mL of deionized water were added into a reactor, dispersed evenly, the temperature was controlled at 5° C., and ultrasonic dispersion was performed for 1 h to obtain a modified gel. Example 8

[0054] A method for preparing a lithium battery separator coating composition comprises the following steps: dissolving 35 g of polyimide in 45 g of deionized water, dispersing the mixture evenly, adding 20 g of the modified gel prepared in Example 4, dispersing the mixture evenly, and obtaining a lithium battery separator coating composition. Example 9

[0055] A method for preparing a lithium battery separator coating composition comprises the following steps: dissolving 35 g of polyimide in 45 g of deionized water, dispersing the mixture evenly, adding 20 g of the modified gel prepared in Example 5, dispersing the mixture evenly, and obtaining a lithium battery separator coating composition. Example 10

[0056] A method for preparing a lithium battery separator coating composition comprises the following steps: dissolving 35 g of polyimide in 45 g of deionized water, dispersing the mixture evenly, adding 20 g of the modified gel prepared in Example 6, dispersing the mixture evenly, and obtaining a lithium battery separator coating composition. Embodiment 11

[0057] A method for preparing a lithium battery separator coating composition comprises the following steps: dissolving 35 g of polyimide in 45 g of deionized water, dispersing the mixture evenly, adding 20 g of the modified gel prepared in Example 7, dispersing the mixture evenly, and obtaining a lithium battery separator coating composition.

[0058] Comparative Example 1

[0059] The preparation method of cellulose aerogel comprises the following steps:

[0060] Add 10 g of sodium hydroxide, 20 g of urea, 140 mL of deionized water, and 4 g of potassium chloride into a reaction bottle and disperse them evenly. Control the temperature at 0°C, add 10 g of cellulose powder, disperse them evenly, centrifuge, let stand, and freeze-dry for 48 hours under the conditions of a cold trap temperature of -60°C and a vacuum degree of -0.1 MPa to obtain cellulose aerogel.

[0061] Comparative Example 2

[0062] The preparation method of the modified gel comprises the following steps:

[0063] S1: 40 g of graphene oxide prepared in Example 1 and 40 mL of deionized water were added to a reaction bottle, dispersed evenly, 10 g of p-phenylenediamine was added, the temperature was controlled at 60° C., the mixture was kept warm for 3 h under stirring, centrifuged, washed, and dried to obtain component 1;

[0064] S2: Add 40g aniline and 80mL 1mol / L hydrochloric acid aqueous solution into the reactor, disperse evenly, add 8g component 1, disperse evenly, add 8g ammonium persulfate, control the temperature to 0°C, keep warm for 6h, wash and dry to obtain modified graphene oxide;

[0065] S3: 25 g of modified graphene oxide, 50 g of cellulose aerogel prepared in Comparative Example 1, and 2500 mL of deionized water were added into a reactor, dispersed evenly, the temperature was controlled at 0° C., and ultrasonic dispersion was performed for 0.5 h to obtain a modified gel.

[0066] Comparative Example 3

[0067] The preparation method of the modified gel comprises the following steps:

[0068] 25 g of graphene oxide, 50 g of the carboxylated cellulose aerogel prepared in Example 2, and 2500 mL of deionized water were added into a reactor, dispersed evenly, and the temperature was controlled at 0° C. Ultrasonic dispersion was performed for 0.5 h to obtain a modified gel.

[0069] Comparative Example 4

[0070] Compared with Example 8, Comparative Example 4 is only that the modified gel prepared in Example 4 added in Example 8 is replaced by the modified gel prepared in Comparative Example 2 in equal amount, and the other components and preparation method are completely consistent with Example 8.

[0071] Comparative Example 5

[0072] Compared with Example 8, in Comparative Example 5, only the modified gel prepared in Example 4 added in Example 8 is replaced by the modified gel prepared in Comparative Example 3 in equal amount, and the other components and preparation method are completely consistent with those in Example 8.

[0073] Performance Testing

[0074] Diaphragm sample material preparation:

[0075] The coating compositions prepared in Examples 8-11 and Comparative Examples 4-5 were respectively coated on both sides of a 25 μm thick microporous Celgard 2325 diaphragm (porosity 41%), with a total coating thickness of 4.5 μm. The coated diaphragms were dried at 60° C. for 24 h to obtain diaphragm materials (Example 8-1, Example 9-1, Example 10-1, Example 11-1, Comparative Example 4-1, Comparative Example 5-1);

[0076] Lithium-ion positive electrode sheet preparation:

[0077] LiCoO2, acetylene black and polyvinylidene fluoride in a mass ratio of 8:1:1 were dispersed in N-methylpyrrolidone and dispersed evenly to obtain a mixed slurry. The mixed slurry was coated on a clean aluminum foil with a thickness of 15 μm, dried in a forced air drying oven at 80°C for 2 h, punched into a circular electrode with a diameter of 10 μm (active material was 2.8 mg), and then vacuum dried at 120°C for 24 h to obtain a positive electrode.

[0078] Battery preparation

[0079] In a glove box filled with gas, the prepared positive electrode sheet is used as the positive electrode, the lithium sheet is used as the negative electrode, 1mol / L LiPF6+EC (ethylene carbonate) / DMC (dimethyl carbonate) / EMC (ethyl methyl carbonate) (volume ratio of 1:1:1) is used as the electrolyte, and the prepared Examples 8-1, 9-1, 10-1, 11-1, Comparative Example 4-1, and Comparative Example 5-1 are respectively assembled into CR032 button batteries with diaphragms, and the batteries are sealed with a sealing machine. The assembled button batteries are placed for 2 hours to fully moisten the electrode sheet and diaphragm for use.

[0080] (1) Mechanical properties of diaphragm: According to GB / T1040.3-2006, the diaphragm with the size of 15cm long × 2cm wide was tested at a speed of 25mm / min. The tensile strength F was calculated as follows:

[0081] F = Fn / (l×d);

[0082] Where: F-tensile strength, MPa; Fn-spline load, N; l-spline length, cm; d-spline width, cm; the test results are shown in Table 1;

[0083] (2) Thermal dimensional stability of the diaphragm: Place the diaphragm with a size of 15 cm long and 4 cm wide in an oven at 120, 130, 140, and 150°C for 0.5 h, then cool it to room temperature naturally and measure and record its length; thermal shrinkage rate A:

[0084] A=[(L0-L) / L0]×100%;

[0085] Where: A-heat shrinkage rate, %; L0-original length of the diaphragm, cm; L-length of the diaphragm after high temperature baking, cm; the test results are shown in Table 1;

[0086] Table 1: Examples 8-1 to 11-1, Comparative Example 4-1, Comparative Example 5-1

[0087] Mechanical properties test data statistics table

[0088]

[0089] It can be seen from Table 1 that the coating prepared in the present application is coated on the surface of the diaphragm, giving the diaphragm high tensile strength and temperature resistance.

[0090] (3) Liquid absorption rate: The weight difference between the material after absorbing the electrolyte and the material before absorption is calculated by the weight method, and the liquid absorption rate η is calculated:

[0091] η=[(W1-W0) / W0]×100%;

[0092] Wherein, η-liquid absorption rate, %; W0-weight of material before adsorption, g; W1-weight of material after adsorption, g; the test results are shown in Table 2;

[0093] (4) Porosity: The porosity of the porous membrane was determined using the n-butanol absorption method. The specific steps were as follows: weigh the mass of the dry material, then soak it in n-butanol for 2 h, wipe off the excess n-butanol on the porous membrane with filter paper and weigh it, and calculate the porosity δ:

[0094] δ = [(M b / ρ b ) / (M p / ρ p +M b / ρ b )]×100%;

[0095] Where, δ-porosity, %; M b -Mass of n-butanol absorbed by the material, g; ρ b -density of n-butanol, g / cm 3 ;M p -Dry mass of material, g; ρ b -Material density, g / cm 3 ; The test results are shown in Table 2;

[0096] (5) Ionic conductivity: The material soaked in electrolyte was sandwiched between two steel sheets (ss), which were used as working electrode and reference electrode respectively. The impedance of the system was measured by AC impedance method on an electrochemical workstation (CHI 660D, Shanghai Chenhua Instrument Co., Ltd.) to obtain the bulk resistance Rb. The detection conditions were 1-10 5 HZ, amplitude 5mV; and calculate the ionic conductivity σ:

[0097] σ = L / (RbA);

[0098] Where, σ-ionic conductivity, mS / cm; L-material thickness, mm; Rb-bulk resistance, Ω; A-test electrode effective contact area, mm 2 ; The test results are shown in Table 2;

[0099] (6) Diaphragm interface resistance test: The test was conducted using the German ZAHNER Zennium electrochemical workstation, using the electrochemical impedance spectroscopy method with a frequency range of 0.1-10 5 HZ, amplitude 5mV; the test results are shown in Table 2;

[0100] Table 2: Performance test data statistics of Examples 8-1 to 11-1, Comparative Example 4-1, and Comparative Example 5-1

[0101]

[0102] It can be seen from Table 2 that the coating prepared in the present application is coated on the surface of the diaphragm, giving the diaphragm good liquid absorption and liquid retention rate, and has high electrical conductivity and low interface resistance.

[0103] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A lithium battery separator coating composition, characterized in that: The invention comprises the following raw materials in weight percentage: 15-35wt% of polyimide, 20-40wt% of modified gel, and 25-65wt% of deionized water, the sum of the raw material components being 100%; The preparation method of the modified gel comprises the following steps: S1: Add graphene oxide and deionized water into a reaction bottle, disperse them evenly, add p-phenylenediamine, control the temperature to 60-70°C, keep warm for 3-6 hours under stirring conditions, centrifuge, wash, and dry to obtain component 1; S2: Add aniline and hydrochloric acid solution into the reaction kettle, disperse evenly, add component 1, disperse evenly, add ammonium persulfate, control the temperature at 0-10°C, keep warm for 6-9h, wash and dry to obtain modified graphene oxide; S3: adding modified graphene oxide, carboxylated cellulose aerogel and deionized water into a reactor, dispersing them evenly, controlling the temperature at 0-5°C, and ultrasonically dispersing them for 0.5-1h to obtain a modified gel; The preparation method of carboxylated cellulose aerogel comprises the following steps: A1: Add sodium hydroxide, urea, deionized water and potassium chloride into a reaction bottle and disperse them evenly, control the temperature at -10 to 0°C, add cellulose powder, disperse them evenly, centrifuge, let stand, and vacuum freeze-dry to obtain cellulose aerogel; A2: Add cellulose aerogel and deionized water into a reaction bottle, disperse them evenly, add TEMPO and sodium bromide, disperse them evenly, adjust the pH to 9-11, add NaClO solution, maintain the pH to 9-11 during the reaction, add anhydrous ethanol to terminate the reaction, wash with water, and dry to obtain carboxylated cellulose aerogel.

2. A lithium battery separator coating composition according to claim 1, characterized in that: The addition ratio of graphene oxide, deionized water, and p-phenylenediamine in S1 is 4 g: 4-40 mL: 1-3 g.

3. A lithium battery separator coating composition according to claim 1, characterized in that: The hydrochloric acid solution in S2 is a 1-1.5 mol / L hydrochloric acid aqueous solution; The addition ratio of aniline, hydrochloric acid solution, component one, and ammonium persulfate is 5 g: 10-12.5 mL: 1-2 g: 1-6 g.

4. A lithium battery separator coating composition according to claim 1, characterized in that: The addition ratio of modified graphene oxide, carboxylated cellulose aerogel, and deionized water in S3 is 0.3-0.5 g: 1 g: 50-100 mL.

5. A lithium battery separator coating composition according to claim 1, characterized in that: The addition ratio of sodium hydroxide, urea, deionized water, potassium chloride and cellulose powder in A1 is 5-10g:10-20g:70-150mL:2-5g:5g.

6. A lithium battery separator coating composition according to claim 1, characterized in that: The NaClO solution in A2 is a 5-10wt% NaClO aqueous solution; the addition ratio of cellulose aerogel, deionized water, TEMPO, sodium bromide, and NaClO solution is 10g: 100-200mL: 0.02-0.05g: 15-30g: 20-30mL.

7. A method for preparing a lithium battery separator coating composition according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: dissolving polyimide in deionized water, dispersing the polyimide uniformly, adding modified gel, dispersing the polyimide uniformly, and obtaining a lithium battery separator coating composition.