Preparation method of ZW890B steel for push-pull rods of economical coal mine hydraulic support

Through component optimization and heat treatment processes, the Ni and Mo content in the hydraulic support push and pull rod is reduced, and combined with two-fire forging and preparatory tissue heat treatment, the saving ZW890B steel is prepared, which solves the problems of high cost and difficult to optimize the performance of traditional push and pull rods. High strength and toughness are achieved while reducing alloy costs.

CN117626129BActive Publication Date: 2024-11-29TANGSHAN ZHIWEI TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311669538.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-07
Publication Date
2024-11-29
Estimated Expiration
2043-12-07

AI Technical Summary

Technical Problem

Due to the high Ni and Mo content of traditional hydraulic support push and pull rods, the alloy costs are high and the mechanical properties are difficult to optimize. The existing technology has failed to effectively reduce costs and meet the requirements of high strength and high toughness.

Method used

Adoption of component optimization design, microstructure design and unique heat treatment process, the Ni and Mo content is reduced by combining smelting, forging and heat treatment processes. Two-fire forging and preparatory tissue heat treatment are used to achieve grain refinement and dense tissue. , and prepared saving ZW890B steel.

Benefits of technology

It achieves the high strength and high toughness requirements of hydraulic support push and pull rods while reducing the alloy cost, ensures the mechanical properties of the material, avoids the phenomenon of coarse grains, and improves the impact toughness of the material through specific heat treatment processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117626129B_ABST
    Figure CN117626129B_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing ZW890B steel for a push-pull rod of an economical coal mine hydraulic support. The specific components of the steel are as follows by mass percentage: C: 0.10-0.18%, Si: 0.20-0.50%, Mn: 0.70-1.50%, P≤0.025%, S≤0.015%, Cr: 0.40-0.90%, Ni: 1.00-1.60%, Mo: 0.20-0.70%, V: 0.03-0.12%, Al: 0.015-0.050%, Cu≤0.20%, O≤20p pm, N: ≤80ppm, H≤1.5ppm, the balance is Fe and inevitable residual impurities; combined with the specific preparation method, the steel for the push-pull rod of the coal mine hydraulic support has uniform structure and fine grains, the grain size is above level 7, the tensile strength is greater than or equal to 900Mpa, the yield strength is ≥800Mpa, the elongation is ≥13%, the cross-sectional shrinkage is ≥46%, and the -20℃ longitudinal low-temperature impact AKv2 is ≥34J. At the same time, the present invention adopts a low Ni and low Mo component design, which effectively reduces the alloy cost and meets the mechanical property requirements of the push-pull rod with a thickness of 100 to 150mm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the fields of steel smelting, steel forging and heat treatment, and in particular relates to a method for preparing ZW890B steel for push-pull rods of economical coal mine hydraulic supports. Background Art

[0002] Hydraulic supports are key equipment for mechanized and process-based coal mining. During coal mining operations, they mainly support coal seams and prevent collapse. When the hydraulic supports need to be moved, the push-pull rods, as key components connecting the scraper, realize the forward and backward movement of large hydraulic supports under the action of hydraulic pressure. With the current large-scale requirements of hydraulic supports, the thickness and width of the push-pull rods are also increasing. In order to meet the mechanical performance requirements, the traditional push-pull rods have a Ni content of not less than 1.40% and a Mo content of not less than 0.45%, and the alloy cost is relatively high.

[0003] Chinese invention patent publication CN116855851A discloses a new HL-grade sucker rod steel and a preparation method thereof, which reduces costs by reducing Ni content and increasing Cr and Mn contents. However, its preparation process does not achieve high performance and low cost by better matching the steel composition. Summary of the invention

[0004] The present invention proposes a method for preparing a ZW890 steel for a push-pull rod for a hydraulic support of a coal mine. The present invention adopts a composition optimization design, a reasonable design of a microstructure and a preparation process, a unique heat treatment process, and a grain refinement treatment technology to ensure that the steel meets the requirements of high strength and high toughness, and produces a ZW890 steel for a push-pull rod for a hydraulic support of a coal mine (because the content of precious alloys such as Ni and Mo can be reduced, the steel becomes a kind of economical steel).

[0005] This is achieved through the following technical means:

[0006] A method for preparing ZW890B steel for push-pull rods of economical coal mine hydraulic supports comprises the following steps:

[0007] I, smelting and casting to obtain a steel ingot, the obtained steel ingot contains, by mass percentage, C: 0.10-0.18%, Si: 0.20-0.50%, Mn: 0.70-1.50%, P≤0.025%, S≤0.015%, Cr: 0.40-0.90%, Ni: 1.00-1.60%, Mo: 0.20-0.70%, V: 0.03-0.12%, Al: 0.015-0.050%, Cu≤0.20%, O≤20ppm, N:≤80ppm, H≤1.5ppm, and the balance is Fe and unavoidable residual impurities.

[0008] II. Forging heating of steel ingot: the steel ingot is charged into the furnace in a cold state, then heated to 820-865℃ and kept warm for 2-5h, then heated to 1200-1230℃ for 4-6h, and then kept warm for 3-5h. After the insulation, it is taken out of the furnace for forging, and a flat anvil is used for direct drawing forging process. The forging is carried out in two fires, and the total forging ratio is 4-7. The first fire forging is for prefabrication and material division. When the forging ratio is left at 1-2, the obtained forging blank is re-charged into the furnace, and the forging blank is reheated to 1100-1230℃ in the furnace and kept warm for 1-2h.

[0009] III. Forging deformation: the forging blank after heat preservation in step II is subjected to the second forging, and is forged and deformed to the finished product size by a direct drawing process, wherein the start forging temperature is controlled at 1100-1230°C, and a small deformation amount of 5%-10% is used for forging during the start forging. When the temperature is reduced to 850-1100°C, a large reduction amount of 15%-25% is used for forging in a single pass. When the temperature is reduced to 750-850°C, a small reduction amount of 5%-10% is used for forging and finishing to the finished product size, so as to refine the internal grains of the workpiece and make the macrostructure dense.

[0010] IV. Preparatory tissue heat treatment: air cool the workpiece after forging in step III for 3 to 10 hours, then heat it to 350 to 450°C and keep it for 2 to 5 hours, then heat it to 850 to 900°C at a rate of 50 to 80°C / h, keep it for 3 to 5 hours, then take it out of the furnace for water quenching to ensure that the surface temperature is not lower than 780°C before entering the water, cool it for 480 to 550 seconds and then take it out of the water, then air cool it for 120 to 150 seconds and then enter the water, then water cool it in water for 120 to 180 seconds and then take it out of the water.

[0011] V, quenching heat treatment: load the workpiece obtained in step IV into a quenching furnace, bundle a thermocouple on the workpiece body after loading, heat the workpiece to 290-310°C and keep it warm for 2-4 hours, then heat it to 780-820°C at a heating rate of 50-80°C / h, keep it warm for 3-5 hours and then take it out of the furnace, then quickly put it into water to ensure that the surface temperature of the workpiece is not lower than 720°C before entering the water, cool it in water to 480-550s and then take it out of the water, air cool it for 120-150s after taking it out of the water and then put it into water again, then water cool it for 120-180s and take it out of the water, perform hardness test after taking it out of the water, if the hardness meets 290-330HB, proceed to the next step, if the hardness does not meet 290-330HB, put it back into the quenching furnace and repeat step V until the hardness reaches 290-330HB.

[0012] VI, tempering heat treatment: the workpiece obtained after the quenching heat treatment in step V is loaded into an electric tempering furnace within 1 to 2 hours of water discharge, heated to a temperature of 200 to 250°C and then kept warm for 4 to 6 hours, then heated to 430 to 450°C at a rate of 20 to 35°C / h and kept warm for 5 to 7 hours. After the insulation is completed, the workpiece is taken out of the furnace and air-cooled to room temperature to obtain ZW890B steel for push-pull rods of economical coal mine hydraulic supports.

[0013] Preferably, the push-pull rod is made of ZW890B steel with the following mass percentage contents: C: 0.14-0.18%, Si: 0.20-0.50%, Mn: 1.35-1.50%, P≤0.020%, S≤0.015%, Cr: 0.70-0.90%, Ni: 1.00-1.20%, Mo: 0.20-0.30%, V: 0.03-0.05%, Al: 0.015-0.050%, Cu≤0.20%, O≤20ppm, N: ≤80ppm, H≤1.5ppm, and the balance is Fe and unavoidable residual impurities.

[0014] Preferably, the push-pull rod is made of ZW890B steel with the following mass percentage contents: C: 0.15-0.18%, Si: 0.35-0.50%, Mn: 1.35-1.45%, P≤0.020%, S≤0.015%, Cr: 0.75-0.85%, Ni: 1.00-1.10%, Mo: 0.20-0.30%, V: 0.03-0.05%, Al: 0.015-0.050%, Cu≤0.20%, O≤20ppm, N: ≤80ppm, H≤1.5ppm, and the balance is Fe and unavoidable residual impurities.

[0015] Preferably, the quenching furnace in step V is a quenching furnace with a control accuracy of ±10°C.

[0016] Preferably, in step VI, the electric tempering furnace is an electric tempering furnace with a temperature control accuracy of ±5°C.

[0017] Preferably, in step V, after loading into the furnace, thermocouples are bundled on the workpiece body, and the bundled thermocouples are evenly distributed at three positions corresponding to the kiln head, the kiln middle and the kiln tail of the quenching furnace (so that the temperature of the workpiece at each position is uniform).

[0018] Preferably, in step II, when the forging ratio remains at 1.5, the obtained forging billet is recharged into the furnace.

[0019] Preferably, after the treatment in step IV, the workpiece obtained has a dense and fine martensitic structure.

[0020] Preferably, in step V, the workpiece obtained in step IV is heated and kept warm to obtain an ultra-fine composite structure.

[0021] Preferably, the smelting and casting to obtain the steel ingot in step I specifically comprises the following steps:

[0022] (1) Electric arc furnace smelting: The raw materials are calculated and proportioned based on the component content of the steel ingot in step I as the component content of the final product. High-clean scrap steel is added to the electric arc furnace, oxygen is blown for 12 to 15 minutes, and a high-draw supplementary blowing operation is adopted. The carbon content of the electric arc furnace is controlled to be 0.14% to 0.16%, and the smelting end temperature is 1620-1650°C. After sampling and testing the carbon content of 0.14% to 0.16% and the phosphorus content of 0.005% to 0.015%, the steel is tapped. During the tapping process, aluminum blocks are added for precipitation deoxidation, and slag-making materials are used for slag washing and alloying, and then the steel is put into the LF furnace for refining.

[0023] (2) LF refining: After the molten steel arrives at the station, it is stirred with argon gas and sent to electric smelting. Aluminum particles and high-purity silicon carbide are used for diffusion deoxidation. The refining time is 60-80 minutes, and the white slag holding time is 20-30 minutes. After the slag is whitened, the chemical composition of the sample is analyzed: C: 0.14-0.18%, Si: 0.20-0.50%, Mn: 1.35-1.50%, P≤0.020%, S≤0.015%, Cr: 0.70-0.90%, Ni: 1.00-1.20%, Mo: 0.20-0.30%, V: 0.03-0.05%, Al: 0.015-0.050%, Cu≤0.20%, and the remainder is Fe and unavoidable residual impurities. Then the package is hoisted to the VD furnace.

[0024] (3) VD refining and casting: After the molten steel arrives at the station, argon gas is introduced for stirring. The VD furnace is pre-evacuated for 4 to 6 minutes. The vacuum is maintained for 20 to 30 minutes at a vacuum degree of ≤67Pa. After the vacuum is broken, 80 to 120 kg of dry alkaline carbon-free covering agent is immediately added to the ladle. Then the temperature is measured, samples are taken, and hydrogen is determined. Then soft blowing is performed until the liquid surface moves slightly and the molten steel is not exposed. The soft blowing time is 15 to 25 minutes. The ladle is hoisted to the ingot casting area for casting to obtain a steel ingot. During the casting process, the superheat of the ladle is controlled between 30 and 50 °C.

[0025] Preferably, the slag-making material in step (1) is a mixture of lime and refined slag, wherein the mass ratio of lime to refined slag is (0.8-1.1):(2.8-3.2) (more preferably 1:3).

[0026] Preferably, the alkaline carbon-free covering agent in step (3) is carbonized rice husk.

[0027] A ZW890B steel for push-pull rods of an economical coal mine hydraulic support is prepared by the above-mentioned preparation method.

[0028] Preferably, the microstructure of the ZW890B steel for the push-pull rod is an undissolved ferrite + tempered troostite structure, wherein the volume proportion of the undissolved ferrite is 10% to 15%.

[0029] An application of ZW890B steel for push-pull rods for economical coal mine hydraulic supports, characterized in that the application is the application of ZW890B steel for push-pull rods for economical coal mine hydraulic supports prepared by the above-mentioned preparation method to manufacture push-pull rods for economical coal mine hydraulic supports.

[0030] The so-called ZW890B in the present invention is the grade name of steel for push-pull rods of economical coal mine hydraulic supports.

[0031] The effects of the present invention are:

[0032] 1. The present invention obtains a dense low-magnification structure by setting a specific forging method, two-fire specific methods and specific forging parameters, so that the original dendrite structure of the steel ingot is broken, and the coarse grain phenomenon is effectively prevented. The specific forging method is combined with the subsequent specific preliminary heat treatment process and sub-temperature quenching process to make the grain size ≥ 7 levels, and at the same time obtain a composite structure of 10% to 15% undissolved ferrite + tempered troostite, so that the final product can improve the impact toughness of the material while ensuring the strength performance.

[0033] 2. The present invention coordinates the steel with specific component content with the specific smelting and subsequent processing technology, so that the processing technology can be more suitable for the steel with the component content of the grade. By reducing the mass percentage content of precious alloy elements such as Ni and Mo, the cost of raw materials is significantly reduced. At the same time, due to the coordination of the process, the mechanical properties of the material are guaranteed to meet the requirements of the final economical steel for push-pull rods of coal mine hydraulic supports.

[0034] 3. The present invention cooperates with the setting of parameters that match the steel grade of the present invention in the entire smelting process, especially by reasonably limiting the parameter settings of LF refining, VD refining and casting processes, and reasonably controlling the gas content (H content ≤ 1.5PPM), thereby ensuring that the finished product has no white spot defects and controlling non-metallic inclusions, so that it can cooperate with subsequent processing technology to achieve the mechanical properties required by the final push-pull rod steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 The metallographic structure of the push-pull rod for the economical coal mine hydraulic support in one embodiment of the present invention is 500 times that of the ZW890B steel.

[0036] Figure 2 This is a grain size diagram of 200 times the ZW890B steel used for push-pull rods of an economical coal mine hydraulic support in one embodiment of the present invention. DETAILED DESCRIPTION

[0037] Example 1

[0038] The push-pull rod specifications of this embodiment are 240×120×3750mm.

[0039] The ingot shape is 400×400mm×L and the ingot weight is 2.3t.

[0040] The composition content of the steel ingot in this embodiment is shown in Table 1. Table 1 shows the composition content of the steel ingot in Example 1.

[0041] Table 1

[0042] Example 1 C Si Mn P S Cr Ni Mo V 0.18wt% 0.42wt% 1.44wt% 0.008wt% 0.003wt% 0.78wt% 1.09wt% 0.21wt% 0.038wt%

[0043] The specific implementation steps after smelting and casting into steel ingots are as follows:

[0044] I. Forging heating of steel ingot: the steel ingot is cold sent to the furnace, kept at 850℃ for 2.5h, then heated to 1230℃ for 4.8h and kept for 3.5h. After the end of the heat preservation, it is taken out of the furnace for forging. The flat anvil is used for direct drawing forging process. The forging is carried out in two fires. The first fire of forging is for prefabrication and material division. A forging ratio of 1.5 is reserved and returned to the furnace for heat preservation. It is returned to the furnace for heat preservation for 1h, and then the second fire of forging in step II is carried out for forming forging.

[0045] II. Forging deformation: Direct drawing process forging deformation to finished product size, forging temperature 1180℃, small deformation during forging, when the temperature drops to 1070℃, large reduction for forging, single pass deformation 22%, when the temperature drops to 820℃, small reduction for finishing to finished product size. Ensure the total forging ratio of 5.3, so that the internal grains of the workpiece are refined and the macrostructure is dense.

[0046] III. Preparatory tissue heat treatment: air-cool the workpiece after forging in step II for 6.5h, then heat it to 400±10℃ and keep it for 2h, then heat it to 880℃ at a rate of 80℃ / h, keep it for 3.5h, take it out of the furnace for quenching, put the forging into water for rapid cooling, the surface temperature before entering the water is 785℃, cool it for 480s and then take it out of the water, then air-cool it for 120s and then put it into water, then water-cool it for 120s and then take it out of the water.

[0047] IV, quenching heat treatment: Load the workpiece obtained in step III into a quenching furnace with a control accuracy of ±10℃. After loading, tie a thermocouple to the workpiece body. The thermocouples are evenly distributed at the head, middle and tail of the furnace to monitor the actual temperature in the furnace. When appropriate, adjust the local temperature according to the set temperature. Keep it at 300±10℃ for 2 hours, heat it to 800℃ at a rate of 50℃ / h, take it out of the furnace after keeping it for 3.5 hours, quickly enter water, the surface temperature before entering the water is 734℃, cool it for 480s and then enter water, then air cool it for 120s and then water cool it for another 120s and then take it out of the water. After taking it out of the water, perform a hardness test. If the hardness meets 310HB, put it into the furnace for tempering heat treatment within 1-2 hours after taking it out of the water.

[0048] V. Tempering: Place the workpiece obtained after the quenching heat treatment in step IV into an electric tempering furnace with a temperature control accuracy of ±5°C, keep it at 250°C for 4 hours, then increase the temperature to 430°C at a rate of 35°C / h and keep it at that temperature for 5 hours. After the insulation is completed, take it out of the furnace and air-cool it to room temperature.

[0049] Results: The grain size of this embodiment is 8.0, the mechanical properties are shown in Table 2, the non-metallic inclusion results are shown in Table 3, the macroscopic low-power structure test results are shown in Table 4, and the microstructure is shown in Table 5. Figure 1 and Figure 2 Table 2 is a table of mechanical properties parameters of the product of Example 1, Table 3 is a table of non-metallic inclusion detection results of Example 1, and Table 4 is a table of macroscopic low-power structure inspection results of Example 1.

[0050] Table 2

[0051] Tensile strength / Mpa Yield strength / Mpa Elongation / % Sectional shrinkage / % -20℃ Impact Energy AKv2 978 865 13.5 58 43.4 / 43.4 / 43.7

[0052] Table 3

[0053]

[0054] Table 4

[0055] Generally loose Loose center Ingot segregation Level 1.5 Level 1.0 Level 0.5

[0056] Example 2

[0057] The push-pull rods of this embodiment have specifications of 250×120×3750 mm. The ingot shape is 400×400 mm×L, and the ingot weight is 2.4 t.

[0058] The composition content of the steel ingot in this embodiment is shown in Table 5, which is a table of the composition content of the steel ingot in Example 2.

[0059] Table 5

[0060] Example 2 C Si Mn P S Cr Ni Mo V 0.15wt% 0.40wt% 1.42wt% 0.007wt% 0.001wt% 0.78wt% 1.08wt% 0.23wt% 0.039wt%

[0061] The specific implementation steps are as follows:

[0062] I. Forging heating of steel ingot: the steel ingot obtained according to the components in Table 5 is cold-charged into the furnace, kept at 850℃ for 2.5h, then heated to 1230℃ for 4.8h and kept for 4h. After the end of the keeping, it is taken out of the furnace for forging, and the flat anvil is used for direct drawing forging process. The forging is carried out in two fires. The first fire of forging is for prefabrication and material division, and a forging ratio of 1.5 is reserved for returning to the furnace for keeping warm. It is returned to the furnace for keeping warm for 1.5h, and then the second fire of forging in step II is carried out for forming forging.

[0063] Ⅱ. Forging deformation: Direct drawing process forging deformation to finished product size, forging temperature 1150℃, small deformation during forging, when the temperature drops to 1065℃, large reduction forging, single pass deformation 20%, when the temperature drops to 830℃, small reduction for finishing to finished product size. Ensure the total forging ratio of 5.2, so that the internal grains of the workpiece are refined and the macrostructure is dense.

[0064] III. Preparatory tissue heat treatment: air-cool the workpiece after forging in step II for 4.5h, then heat it to 400±10℃ and keep it for 2h, then heat it to 880℃ at a rate of 80℃ / h, keep it for 3.5h, take it out of the furnace for quenching, put the forging into water for rapid cooling, the surface temperature before entering the water is 790℃, cool it for 480s and then take it out of the water, then air-cool it for 120s and then put it into water, then water-cool it for 120s and then take it out of the water.

[0065] IV, quenching heat treatment: Load the workpiece obtained in step III into a quenching furnace with a control accuracy of ±10℃. After loading, tie a thermocouple to the workpiece body. The thermocouples are evenly distributed at the head, middle and tail of the furnace to monitor the actual temperature in the furnace. When appropriate, adjust the local temperature according to the set temperature. Keep it at 300℃±10 for 2 hours, heat it to 810℃ at a rate of 50℃ / h, take it out of the furnace after keeping it for 3.5 hours, quickly enter water, the surface temperature before entering the water is 728℃, cool it for 480s and then enter water, then air cool it for 120s and then water cool it for another 120s and then take it out of the water. After taking it out of the water, perform a hardness test. The hardness meets 315HB. Put it into the furnace for tempering heat treatment within 1-2 hours after taking it out of the water.

[0066] V. Tempering: Place the workpiece obtained after the quenching heat treatment in step IV into an electric tempering furnace with a temperature control accuracy of ±5°C, keep it at 250°C for 4 hours, then increase the temperature to 430°C at a rate of 35°C / h and keep it at that temperature for 5 hours. After the insulation is completed, take it out of the furnace and air-cool it to room temperature.

[0067] The results of the present embodiment show that the grain size is 8.0, the mechanical properties are shown in Table 6, the non-metallic inclusion results are shown in Table 7, and the macroscopic low-power structure inspection results are shown in Table 8. Table 6 is a table of mechanical properties parameters of the product of Example 2, Table 7 is a table of non-metallic inclusion inspection results of Example 2, and Table 8 is a table of macroscopic low-power structure inspection results of Example 2.

[0068] Table 6

[0069] Tensile strength / Mpa Yield strength / Mpa Elongation / % Sectional shrinkage / % -20℃ Impact Energy AKv2 954 830 15.8 61 47.8 / 50.9 / 63

[0070] Table 7

[0071]

[0072] Table 8

[0073] Generally loose Loose center Ingot segregation Level 1.5 Level 1.5 Level 1.0

[0074] Example 3

[0075] First, prepare the steel ingot, using the following steps:

[0076] (1) Electric arc furnace smelting: The raw material ratio is calculated based on the component contents in Table 9 as the component contents of the final product (except for the content of each element in Table 9, Al is limited to 0.025wt.%, Cu is 0.06wt.%, O is 13ppm, N is 56ppm, H is 1.1ppm, and the balance is Fe and inevitable residual impurities). High-clean scrap steel is added to the electric arc furnace, oxygen is blown for 13min, and high-draw supplementary blowing operation is adopted. The carbon content of the electric furnace is controlled to be 0.15wt.%, and the smelting end temperature is 1645°C. The carbon content of the sample is 0.15wt.% and the phosphorus content is 0.006wt.% before tapping. During the tapping process, aluminum blocks are added for precipitation deoxidation, and slag-making materials are used for slag washing and alloying, and then the steel is put into the LF furnace for refining.

[0077] (2) LF refining: After the molten steel arrives at the station, it is stirred with argon gas and sent to electric smelting. Aluminum particles and high-purity silicon carbide are used for diffusion deoxidation. The refining time is 68 minutes, and the white slag is kept for 26 minutes. After the slag is white, samples are taken for chemical composition analysis, and then the bag is hoisted to the VD furnace.

[0078] (3) VD refining and casting: After the molten steel arrives at the station, argon gas is introduced for stirring. The VD furnace is pre-evacuated for 5 minutes. At a vacuum degree of ≤67Pa, the vacuum degree is maintained for 25 minutes. Immediately after the vacuum is broken, 92kg of dry alkaline carbon-free covering agent is added to the ladle. Then the temperature is measured, sampling is performed, and hydrogen is determined. Then soft blowing is performed until the liquid surface moves slightly and the molten steel is not exposed. The soft blowing time is 20 minutes. The ladle is hoisted to the ingot casting area for casting to obtain a steel ingot. During the casting process, the superheat of the ladle is controlled between 30 and 40°C.

[0079] The push-pull rod specifications of this embodiment are 270×130×4100mm; the ingot shape is: 500×500mm×L, and the ingot weight is 3t.

[0080] The composition content of the steel ingot in this embodiment is shown in Table 9, which is a table of the composition content of the steel ingot in Example 3.

[0081] Table 9

[0082] Example 3 C Si Mn P S Cr Ni Mo V 0.15wt% 0.40wt% 1.38wt% 0.006wt% 0.001wt% 0.78wt% 1.00wt% 0.20wt% 0.040wt%

[0083] The specific implementation steps are as follows:

[0084] I. Forging heating of steel ingot: the steel ingot is cold sent to the furnace, kept at 850℃ for 3h, then heated to 1230℃ for 4.8h and kept for 5h. After the end of the keeping, it is taken out of the furnace for forging. The flat anvil is used for direct drawing forging process. The forging is carried out in two fires. The first fire of forging is for prefabrication and material division. A forging ratio of 1.5 is reserved and returned to the furnace for keeping warm. It is returned to the furnace for keeping warm for 1.5h, and then the second fire of forging in step II is carried out for forming forging.

[0085] Ⅱ. Forging deformation: Direct drawing process forging deformation to finished product size, forging temperature 1170℃, small deformation during forging, when the temperature drops to 1055℃, large reduction forging, single pass deformation 21%, when the temperature drops to 815℃, small reduction for finishing to finished product size. Ensure the total forging ratio of 7.1, so that the internal grains of the workpiece are refined and the low-magnification structure is dense.

[0086] III. Preparatory tissue heat treatment: air cool the workpiece after forging in step II for 5h, then heat it to 400±10℃ and keep it for 2h, then heat it to 880℃ at a rate of 80℃ / h, keep it for 3.7h, take it out of the furnace for quenching, put the forging into water for rapid cooling, the surface temperature before entering the water is 782℃, cool it for 480s and then take it out of the water, then air cool it for 120s and then put it into water, then water cool it for 180s and then take it out of the water.

[0087] IV, quenching heat treatment: Load the workpiece obtained in step III into a quenching furnace with a control accuracy of ±10℃. After loading, tie a thermocouple to the workpiece body. The thermocouples are evenly distributed at the head, middle and tail of the furnace to monitor the actual temperature in the furnace. When appropriate, adjust the local temperature according to the set temperature. Keep it at 300±10℃ for 2 hours, heat it to 805℃ at a rate of 50℃ / h, take it out of the furnace after keeping it for 4.5 hours, quickly enter water, and the surface temperature before entering the water is 731℃. Cool it for 480s and then exit the water. Air cool it for 120s and then enter the water. Then water cool it for 180s and exit the water. After exiting the water, perform a hardness test. The hardness meets 315HB. Load it into the furnace for tempering heat treatment within 1-2 hours after exiting the water.

[0088] V. Tempering: Place the workpiece obtained after the quenching heat treatment in step IV into an electric tempering furnace with a temperature control accuracy of ±5°C, keep it at 250°C for 4 hours, then heat it to 430°C at a rate of 35°C / h and keep it at that temperature for 5.4 hours. After the insulation is completed, take it out of the furnace and air-cool it to room temperature.

[0089] The results of the present embodiment show that the grain size is 7.5, the mechanical properties are shown in Table 10, the non-metallic inclusion results are shown in Table 11, and the macroscopic low-power structure inspection results are shown in Table 12. Table 10 is a table of mechanical properties parameters of the product of Example 3, Table 11 is a table of non-metallic inclusion inspection results of Example 3, and Table 12 is a table of macroscopic low-power structure inspection results of Example 3.

[0090] Table 10

[0091] Tensile strength / Mpa Yield strength / Mpa Elongation / % Sectional shrinkage / % -20℃ Impact Energy AKv2 1037 927 15 66 39.5 / 51.4 / 58

[0092] Table 11

[0093]

[0094] Table 12

[0095] Generally loose Loose center Ingot segregation Level 1.0 Level 1.0 Level 0

[0096] Comparative Example 1

[0097] In the forging process of this comparative example, the second forging ratio is 0.5, and no preparatory structure heat treatment is used, and a conventional one-step complete austenitization quenching is used followed by a tempering process. The other settings (steel component content and smelting, casting, etc.) are the same as those in Example 1. By testing and observing the microstructure of the obtained product, it is found that the grain size is 4-6, the structure is tempered troostite, and its mechanical properties are shown in Table 13, which is a mechanical property parameter table of the product of Comparative Example 1. By comparing the data in Table 13 with those in Table 2, it is explained that the specific two-fire forging and preparatory structure heat treatment set by the present invention, as well as the quenching and tempering process with specific parameters in specific steps and specific steel components and smelting methods are the optimal solutions.

[0098] Table 13

[0099] Tensile strength / Mpa Yield strength / Mpa Elongation / % Sectional shrinkage / % -20℃ Impact Energy AKv2 966 860 16 59 11.5 / 17 / 16

[0100] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing ZW890B steel for push-pull rods of economical coal mine hydraulic supports, characterized in that: The steps include: I, smelting and casting to obtain a steel ingot, wherein the obtained steel ingot has the following contents by mass percentage: C: 0.10-0.18%, Si: 0.20-0.50%, Mn: 0.70-1.50%, P≤0.025%, S≤0.015%, Cr: 0.40-0.90%, Ni: 1.00-1.60%, Mo: 0.20-0.70%, V: 0.03-0.12%, Al: 0.015-0.050%, Cu≤0.20%, O≤20ppm, N:≤80ppm, H≤1.5ppm, and the balance is Fe and unavoidable residual impurities; II. Forging heating of steel ingot: the steel ingot is sent to the furnace in a cold state, and then heated to 820~865℃ and kept warm for 2~5h, and then heated to 1200~1230℃ for 4~6h, and then kept warm for 3~5h. After the end of the heat preservation, it is taken out of the furnace for forging, and a flat anvil is used for direct drawing forging process. The forging is carried out in two fires, and the total forging ratio is 4~7. The first fire forging is for prefabrication and material division. When the forging ratio is left at 1.5~2, the forging blank is re-charged into the furnace, and the forging blank is reheated to 1100~1230℃ in the furnace and kept warm for 1~2h. III. Forging deformation: the forging blank after heat preservation in step II is subjected to the second forging, and is forged and deformed to the finished product size by a direct drawing process, wherein the forging temperature is controlled at 1100-1230°C, and a small deformation of 5%-10% is used for forging during the forging. When the temperature is reduced to 850-1100°C, a large reduction of 15%-25% is used for forging in a single pass. When the temperature is reduced to 750-850°C, a small reduction of 5%-10% is used for forging and finishing to the finished product size, so that the internal grains of the workpiece are refined and the macrostructure is dense; IV. Preparatory tissue heat treatment: air cool the workpiece after forging in step III for 3-10 hours, then heat it to 350-450℃ and keep it for 2-5 hours, then heat it to 850-900℃ at a rate of 50-80℃ / h, keep it for 3-5 hours, then take it out of the furnace for water quenching, ensuring that the surface temperature is not lower than 780℃ before entering the water, cool it for 480-550s and then take it out of the water, then air cool it for 120-150s and then enter the water, then water cool it in the water for 120-180s and then take it out of the water; V, quenching heat treatment: load the workpiece obtained in step IV into a quenching furnace, tie a thermocouple to the workpiece body after loading, heat the workpiece to 290~310℃ and keep it warm for 2~4 hours, then heat it to 780~820℃ at a heating rate of 50~80℃ / h, keep it warm for 3~5h and then take it out of the furnace, then quickly put it into water to ensure that the surface temperature of the workpiece is not lower than 720℃ before entering the water, cool it in water for 480~550s and then take it out of the water, air cool it for 120~150s after taking it out of the water and then put it into water again, then water cool it for 120~180s and then take it out of the water, perform hardness test after taking it out of the water, if the hardness meets 290~330HB, proceed to the next step, if the hardness does not meet 290~330HB, transfer it back to the quenching furnace and repeat step V until the hardness reaches 290~330HB; VI. Tempering heat treatment: the workpiece obtained after the quenching heat treatment in step V is loaded into an electric tempering furnace within 1-2 hours of exiting the water, heated to a temperature of 200-250°C and then kept warm for 4-6 hours, then heated to 430-450°C at a rate of 20-35°C / h and kept warm for 5-7 hours. After the insulation is completed, the workpiece is taken out of the furnace and air-cooled to room temperature to obtain ZW890B steel for push-pull rods of economical coal mine hydraulic supports.

2. The method for preparing ZW890B steel for push-pull rods of economical coal mine hydraulic supports according to claim 1, characterized in that: The ZW890B steel for the push-pull rod has the following mass percentage contents: C: 0.14-0.18%, Si: 0.20-0.50%, Mn: 1.35-1.50%, P≤0.020%, S≤0.015%, Cr: 0.70-0.90%, Ni: 1.00-1.20%, Mo: 0.20-0.30%, V: 0.03-0.05%, Al: 0.015-0.050%, Cu≤0.20%, O≤20ppm, N: ≤80ppm, H≤1.5ppm, and the remainder is Fe and unavoidable residual impurities.

3. The method for preparing ZW890B steel for push-pull rods of economical coal mine hydraulic supports according to claim 1, characterized in that: The quenching furnace described in step V is a quenching furnace with a control accuracy of ±10°C; in step VI, the electric tempering furnace is an electric tempering furnace with a temperature control accuracy of ±5°C; in step V, after the furnace is loaded, thermocouples are bundled on the workpiece body, and the bundled thermocouples are evenly distributed at three positions corresponding to the kiln head, kiln middle and kiln tail of the quenching furnace.

4. The method for preparing ZW890B steel for push-pull rods of economical coal mine hydraulic supports according to claim 1, characterized in that: In step II, when the forging ratio remains at 1.5, the obtained forging billet is recharged into the furnace.

5. The method for preparing ZW890B steel for push-pull rods of economical coal mine hydraulic supports according to claim 3, characterized in that: After the treatment in step IV, the obtained workpiece has a dense and fine martensite structure.

6. The method for preparing ZW890B steel for push-pull rods of economical coal mine hydraulic supports according to claim 1, characterized in that: The smelting and casting to obtain the steel ingot in step I specifically comprises the following steps: (1) Electric arc furnace smelting: The raw material ratio is calculated based on the component content of the steel ingot in step I as the component content of the final product. High-clean scrap steel is added to the electric arc furnace, oxygen is blown for 12-15 minutes, and a high-draw supplementary blowing operation is adopted. The carbon content of the electric arc furnace is controlled to be 0.14%-0.16%, and the smelting end temperature is 1620-1650°C. After sampling and testing the carbon content of 0.14%-0.16% and the phosphorus content of 0.005%-0.015%, the steel is tapped. During the tapping process, aluminum blocks are added for precipitation deoxidation, and slag-making materials are added for slag washing and alloying, and then the steel is put into the LF furnace for refining; (2) LF refining: After the molten steel arrives at the station, it is stirred with argon gas and sent to electric smelting. Aluminum particles and high-purity silicon carbide are used for diffusion deoxidation. The refining time is 60~80min, and the white slag holding time is 20~30min. After the slag is whitened, the chemical composition of the sample is analyzed to meet the requirements of C: 0.14~0.18%, Si: 0.20~0.50%, Mn: 1.35~1.50%, P≤0.020%, S≤0.015%, Cr: 0.70~0.90%, Ni: 1.00~1.20%, Mo: 0.20~0.30%, V: 0.03~0.05%, Al: 0.015~0.050%, Cu≤0.20%, and then the ladle is hoisted to the VD furnace; (3) VD refining and casting: After the molten steel arrives at the station, argon gas is introduced for stirring. The VD furnace is pre-evacuated for 4 to 6 minutes. The vacuum is maintained at ≤67Pa for 20 to 30 minutes. After the vacuum is broken, 80 to 120 kg of dry alkaline carbon-free covering agent is immediately added to the ladle. The temperature is then measured and maintained at 1550 to 1580°C. Samples are taken and the hydrogen content is determined to be ≤1.5 PPM. Soft blowing is then performed with the liquid surface moving slightly and the molten steel not exposed. The soft blowing time is 15 to 25 minutes. The ladle is then hoisted to the ingot casting area for casting to obtain a steel ingot. During the casting process, the superheat of the ladle is controlled between 30 and 50°C.

7. The method for preparing ZW890B steel for push-pull rods of economical coal mine hydraulic supports according to claim 6, characterized in that: The slag-making material in step (1) is a mixture of lime and refined slag, wherein the mass ratio of lime to refined slag is (0.8-1.1):(2.8-3.2); the alkaline carbon-free covering agent in step (3) is carbonized rice husk.

8. A ZW890B steel for push-pull rods of economical coal mine hydraulic supports, characterized in that: The push-pull rod is made of ZW890B steel using the preparation method described in any one of claims 1 to 7.

9. The ZW890B steel for push-pull rods of the economical coal mine hydraulic support according to claim 8 is characterized in that: The microstructure of the ZW890B steel for the push-pull rod is an undissolved ferrite + tempered troostite structure, wherein the volume proportion of the undissolved ferrite is 10% to 15%.

10. Application of ZW890B steel for push-pull rods of economical coal mine hydraulic supports, characterized in that: The application is the use of ZW890B steel for economical coal mine hydraulic support push-pull rods prepared by the preparation method described in any one of claims 1 to 7 to manufacture economical coal mine hydraulic support push-pull rods.

Citation Information

Patent Citations

  • HL-grade novel sucker rod steel and preparation method thereof

    CN116855851A

  • Preparation method of high-toughness and high-isotropy ZW868 hot work die steel

    CN107488813A

  • Nb-containing ZW633 large-sized plastic die steel for die core and preparation method of Nb-containing ZW633 large-sized plastic die steel

    CN107699800A