Packaging process of mobile storage device
By combining alumina surface modification and acrylic modified epoxy resin, the modified resin glue is prepared, which solves the problem of insufficient flexibility and thermal conductivity of epoxy resin and alumina composite adhesive under high crosslinking. A significant improvement in thermal conductivity and peel strength has been achieved.
Patent Information
- Application Number
- CN202311671341.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-07
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-12-07
AI Technical Summary
The existing composite adhesives of epoxy resin and alumina are poorly flexible, brittle, and have insufficient thermal conductivity under high crosslinking. The alumina has poor compatibility with organic resins, resulting in increased viscosity and increased interface thermal resistance, which is difficult to Meets thermal conductivity and fluidity requirements.
By surface modification of alumina and modification of epoxy resin with acrylic acid, the preparation process of modified resin glue is designed, including heating and drying, high-speed stirring, heating and melting, and adding modified BN and modified fillers in batches. , uniform stirring is performed using a curing agent and a solvent to form a modified resin glue to improve thermal conductivity and peel strength.
It significantly improves the thermal conductivity and peel strength of the resin glue, optimizes the dispersion of fillers, reduces viscosity, meets the thermal conductivity and fluidity requirements, and enhances the stability and performance of the product.
Smart Images

Figure BDA0004593319680000141 
Figure BDA0004593319680000151
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of mobile storage devices and relates to a packaging process of a mobile storage device. Background Art
[0002] Epoxy resin molecules contain active groups such as epoxy groups, ether bonds and hydroxyl groups, which give them excellent cohesive strength. In addition, epoxy resins also show excellent high temperature resistance, chemical resistance and bonding properties. However, under high cross-linking conditions, defects such as poor flexibility and high brittleness may occur. In order to give full play to the advantages of epoxy resin and acrylic acid and make up for each other's shortcomings, we use acrylic acid to modify epoxy resin. This not only improves heat resistance and water resistance, but also enhances properties such as high mechanical strength.
[0003] Alumina has unique advantages in thermal conductivity and insulation, and is often used as an important filler in thermally conductive and insulating adhesives. However, the surface polarity of alumina is relatively strong, and its compatibility with the organic resin matrix is poor. Alumina particles are easy to agglomerate and difficult to disperse evenly in the polymer. In addition, the thermal conductivity of alumina fillers themselves is not high. In order to prepare adhesives with good thermal conductivity, we usually increase the filling amount. However, high filling will increase the viscosity of the composite adhesive, making it difficult to meet the fluidity requirements, and may also reduce the mechanical properties of the composite adhesive. In addition, there is a difference in surface tension between alumina and organic resins, which makes it difficult for the resin matrix to wet the particle surface, thereby introducing voids at the interface, resulting in an increase in the interfacial thermal resistance of the composite adhesive. In order to improve the compatibility between alumina and the resin matrix, we need to perform surface modification on alumina. Summary of the invention
[0004] The purpose of the present invention is to provide a packaging process for a mobile storage device. The present invention significantly improves the thermal conductivity and peel strength of the resin glue by modifying the filler, reducing the viscosity of the resin material system, and promoting the dispersion of the filler in the system.
[0005] The purpose of the present invention can be achieved by the following technical solutions:
[0006] A packaging process for a mobile storage device, the packaging process comprising the following steps:
[0007] 1) Preliminarily fix the controller, electrical components and storage chips on the substrate by resin glue;
[0008] 2) Solder the controller, electrical components, and storage chip to the substrate using solder paste;
[0009] 3) welding gold wires between the memory chip, the controller, the electrical components and the upper surface of the substrate, and performing reflow soldering to obtain a semi-finished product;
[0010] 4) Check the welding condition of semi-finished products, and conduct H2 test on the semi-finished products after welding;
[0011] 5) After the H2 test is completed, the shell is assembled, the outer surface of the shell is laser engraved, and then it is packaged to complete the processing.
[0012] As a preferred technical solution of the present invention, the parameters of the laser carving are a laser wavelength of 400-3500nm, a power of 5-12W, a frequency of 0.1-220KHz, a laser routing speed of 0.01-50000mm / s, and a filling spacing of 0.01-6mm.
[0013] As a preferred technical solution of the present invention, the surface of the substrate contains a metal film layer, and the metal film layer contains one or more of the elements Cu, Ni, Zn and Ti.
[0014] As a preferred technical solution of the present invention, the method for preparing the resin glue comprises the following steps:
[0015] S1, heating and drying the mixed filler, adding a coupling agent and stirring at high speed to obtain a modified filler;
[0016] S2, heating and melting the epoxy resin, adding the mixture and stirring and mixing, adding acrylic acid and a catalyst and heating treatment, adding modified BN and modified filler in batches and stirring and mixing, to obtain a prefabricated material;
[0017] S3, adding curing agent and solvent to the prefabricated material, stirring evenly, and curing to obtain resin glue.
[0018] As a preferred technical solution of the present invention, in step S1, the heating and drying conditions are 70-80°C and drying for 2-2.5h; the high-speed stirring conditions are 1000-1200r / min and stirring and mixing for 30-45min; the mixed filler is a mixture of three fillers with a particle size ratio of 12:5:1.5 and a weight ratio of 5:3:2; the filler is alumina; the mass ratio of the mixed filler to the coupling agent is 15:1; the coupling agent is one or both of a silane coupling agent and a titanate coupling agent.
[0019] As a preferred technical solution of the present invention, in step S2, the heating and melting temperature is 90-95°C; the condition for adding in batches is to add in 4 batches of equal amounts; the condition for the temperature treatment is to heat to 105-115°C and keep warm for 1.5 hours; the condition for stirring and mixing is to stir and mix at 90°C for 15-20 minutes; the mixture is formed by mixing hydroquinone and p-hydroxyanisole in a mass ratio of 3:2; the catalyst is triphenylphosphine; the mass ratio of the epoxy resin, the mixture, acrylic acid, the catalyst, the modified BN and the modified filler is 30:0.40-0.45:10:0.37-0.42:20-22:60-65.
[0020] As a preferred technical solution of the present invention, in step S3, the uniform stirring time is 2-3h; the mass ratio of the prefabricated material, the curing agent and the solvent is 100:1.5-1.8:25; the curing agent is a mixture of 2-methylimidazole and dicyandiamide in a mass ratio of 1:3; and the solvent is 2-butanone.
[0021] As a preferred technical solution of the present invention, in step S2, the preparation method of the modified BN comprises the following steps:
[0022] S11, stirring and mixing the silane coupling agent, ethanol and deionized water to obtain a mixed solution;
[0023] S12, dispersing BN in an alkaline solution and subjecting it to ultrasonic treatment, centrifuging to obtain a solid, adding it to the mixed solution for heating reaction, centrifuging to obtain a solid, and drying it to obtain a preform;
[0024] S13, mixing the preform, toluene and perhydropolysilazane, subjecting the mixture to ultrasonic reaction, centrifuging to remove toluene, and drying to obtain modified BN.
[0025] As a preferred technical solution of the present invention, in step S11, the silane coupling agent is silane coupling agent KH570; the mass ratio of the silane coupling agent, ethanol and deionized water is 2:70:25; in step S12, the alkaline solution is a sodium hydroxide aqueous solution with a mass concentration of 12%; the mass ratio of BN to the sodium hydroxide aqueous solution is 1:9.0-9.5; the conditions of the ultrasonic treatment are 70-75°C and ultrasonic treatment for 3.2-3.8h; the conditions of the heating reaction are 60-65°C and reaction for 3h; the mass ratio of BN to the mixed solution is 1:1.0-1.5.
[0026] As a preferred technical solution of the present invention, in step S13, the mass ratio of the preform, toluene and perhydropolysilazane is 1.0-1.2:100:2.2; the conditions of the ultrasonic reaction are 60°C for 2 hours; and the conditions of the drying are 2.45 GHz microwave frequency for 5 minutes and 65-70°C for 10 hours.
[0027] Beneficial effects of the present invention:
[0028] (1) The present invention solders the components to the base and initially fixes them with resin glue, which provides good thermal conductivity. The reflow soldering process is designed to ensure effective soldering of the gold wire and consistency of the product soldering quality.
[0029] (2) By compounding alumina particles of different sizes, the stacking of mixed fillers can be optimized to form a more compact structure, thereby promoting the formation of a thermal conductive path and significantly improving the thermal conductivity of the resin system.
[0030] (3) Boron nitride is modified by sodium hydroxide and a coupling agent so that its surface hydroxyl groups react with polysilazane to obtain modified boron nitride. This modified boron nitride can be effectively dispersed in an organic solvent and significantly improves the peel strength of the material, further improving the thermal conductivity of the boron nitride-filled epoxy resin material.
[0031] (4) Through the ring-opening esterification reaction of epoxy resin with acrylic acid, under the action of catalyst and mixture, the viscosity of the resin system can be effectively reduced and the dispersion of fillers in the resin system can be promoted. At the same time, the modification of epoxy resin with acrylic acid can significantly improve the thermal conductivity and peel strength of epoxy resin.
[0032] (5) Using the compound mixture as an inhibitor can synergistically enhance the inhibitory effect, significantly improve the storage stability of the resin, and basically avoid the occurrence of gelation. In contrast, the inhibitor alone has a relatively poor inhibitory effect and a weak ability to inhibit the polymerization of epoxy resin itself, which is not conducive to the reaction of acrylic acid with epoxy resin. DETAILED DESCRIPTION
[0033] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.
[0034] A packaging process for a mobile storage device, the packaging process comprising the following steps:
[0035] 1) The controller, the electrical components and the memory chip are initially fixed on the substrate by resin glue; wherein the surface of the substrate contains a metal film layer, and the metal film layer contains one or more of Cu element, Ni element, Zn element and Ti element.
[0036] 2) Solder the controller, electrical components, and storage chip to the substrate using solder paste;
[0037] 3) welding gold wires between the memory chip, the controller, the electrical components and the upper surface of the substrate, and performing reflow soldering to obtain a semi-finished product;
[0038] 4) Check the welding condition of semi-finished products, and conduct H2 test on the semi-finished products after welding;
[0039] 5) After completing the H2 test, the shell is assembled, and the outer surface of the shell is laser engraved and then packaged to complete the processing; wherein the parameters of the laser engraving are a laser wavelength of 400-3500nm, a power of 5-12W, a frequency of 0.1-220KHz, a laser routing speed of 0.01-50000mm / s, and a filling spacing of 0.01-6mm.
[0040] Example 1
[0041] The preparation method of the resin glue comprises the following steps:
[0042] S1. After heating and drying the mixed filler, a coupling agent is added and stirred at high speed to obtain a modified filler; wherein the heating and drying conditions are drying at 70°C for 2 hours; the high-speed stirring conditions are stirring and mixing at 1000 r / min for 30 minutes; the mixed filler is a mixture of three types of alumina with a particle size ratio of 12:5:1.5 and a weight ratio of 5:3:2; the mass ratio of the mixed filler to the silane coupling agent KH560 is 15:1;
[0043] S2, heating and melting the epoxy resin, adding the mixture to stir and mix, adding acrylic acid and triphenylphosphine and heating treatment, adding modified BN and modified filler in batches and stirring and mixing to obtain a prefabricated material; wherein the heating and melting temperature is 90°C; the condition of adding in batches is to add in 4 batches in equal amounts; the condition of heating treatment is to heat to 105°C and keep warm for 1.5h; the condition of stirring and mixing is to stir and mix at 90°C for 15min; the mixture is mixed by hydroquinone and p-hydroxyanisole in a mass ratio of 3:2;
[0044] The mass ratio of the epoxy resin, the mixture, acrylic acid, triphenylphosphine, modified BN and modified filler is 30:0.40:10:0.37:20:60:
[0045] S3, adding curing agent and 2-butanone to the prefabricated material and stirring evenly, and then curing to obtain resin glue; wherein the stirring time is 2h;
[0046] The mass ratio of the prefabricated material, the curing agent and the solvent is 100:1.5:25; the curing agent is a mixture of 2-methylimidazole and dicyandiamide in a mass ratio of 1:3;
[0047] The preparation method of the modified BN comprises the following steps:
[0048] S11, stirring and mixing silane coupling agent KH570, ethanol and deionized water to obtain a mixed solution; wherein the mass ratio of the silane coupling agent KH570, ethanol and deionized water is 2:70:25;
[0049] S12, dispersing BN in an alkaline solution and performing ultrasonic treatment, centrifugally separating and taking out a solid, adding the solid to the mixed solution for heating reaction, centrifugally separating and taking out the solid for drying to obtain a preform; wherein the alkaline solution is a sodium hydroxide aqueous solution with a mass concentration of 12%; the mass ratio of BN to the sodium hydroxide aqueous solution is 1:9.0; the conditions of the ultrasonic treatment are 70° C. and ultrasonic treatment for 3.2 h; the conditions of the heating reaction are 60° C. and reaction for 3 h; the mass ratio of BN to the mixed solution is 1:1.0;
[0050] S13, after mixing the preform, toluene and perhydropolysilazane, after ultrasonic reaction, after centrifugal separation to remove the toluene, after drying, to obtain modified BN; wherein the mass ratio of the preform, toluene and perhydropolysilazane is 1.0:100:2.2; the conditions of the ultrasonic reaction are at a temperature of 60°C and a reaction time of 2h; the conditions of the drying are at a microwave frequency of 2.45GHz, a treatment time of 5min, a temperature of 65°C, and a drying time of 10h.
[0051] Example 2
[0052] The preparation method of the resin glue comprises the following steps:
[0053] S1. After heating and drying the mixed filler, a coupling agent is added and stirred at high speed to obtain a modified filler; wherein the heating and drying conditions are at a temperature of 72°C and drying for 2.1 hours; the high-speed stirring conditions are at 1040 r / min and stirring and mixing for 33 minutes; the mixed filler is a mixture of three types of alumina with a particle size ratio of 12:5:1.5 and a weight ratio of 5:3:2; the mass ratio of the mixed filler to the silane coupling agent KH560 is 15:1;
[0054] S2, heating and melting the epoxy resin, adding the mixture to stir and mix, adding acrylic acid and triphenylphosphine and heating treatment, adding modified BN and modified filler in batches and stirring and mixing to obtain a prefabricated material; wherein the heating and melting temperature is 91°C; the condition of adding in batches is to add in equal amounts in 4 batches; the condition of heating treatment is to heat to 107°C and keep warm for 1.5h; the condition of stirring and mixing is to stir and mix at 90°C for 16min; the mixture is mixed by hydroquinone and p-hydroxyanisole in a mass ratio of 3:2;
[0055] The mass ratio of the epoxy resin, the mixture, acrylic acid, triphenylphosphine, modified BN and modified filler is 30:0.41:10:0.38:20.4:61;
[0056] S3, adding curing agent and 2-butanone to the prefabricated material and stirring evenly, and then curing to obtain resin glue; wherein the stirring time is 2.2h;
[0057] The mass ratio of the prefabricated material, the curing agent and the solvent is 100:1.56:25; the curing agent is a mixture of 2-methylimidazole and dicyandiamide in a mass ratio of 1:3;
[0058] The preparation method of the modified BN comprises the following steps:
[0059] S11, stirring and mixing silane coupling agent KH570, ethanol and deionized water to obtain a mixed solution; wherein the mass ratio of the silane coupling agent KH570, ethanol and deionized water is 2:70:25;
[0060] S12, dispersing BN in an alkaline solution and performing ultrasonic treatment, centrifugally separating and taking out a solid, adding the solid to the mixed solution for heating reaction, centrifugally separating and taking out the solid for drying to obtain a preform; wherein the alkaline solution is a sodium hydroxide aqueous solution with a mass concentration of 12%; the mass ratio of BN to the sodium hydroxide aqueous solution is 1:9.1; the conditions of the ultrasonic treatment are 71° C. and ultrasonic treatment for 3.3 h; the conditions of the heating reaction are 61° C. and reaction for 3 h; the mass ratio of BN to the mixed solution is 1:1.1;
[0061] S13. After mixing the preform, toluene and perhydropolysilazane, subjecting them to ultrasonic reaction, centrifuging to remove the toluene and drying to obtain modified BN; wherein the mass ratio of the preform, toluene and perhydropolysilazane is 1.04:100:2.2; the ultrasonic reaction conditions are 60°C for 2h; the drying conditions are 2.45GHz microwave frequency for 5min, 66°C for 10h.
[0062] Example 3
[0063] The preparation method of the resin glue comprises the following steps:
[0064] S1. After heating and drying the mixed filler, a coupling agent is added and stirred at high speed to obtain a modified filler; wherein the heating and drying conditions are at a temperature of 74°C and drying for 2.2 hours; the high-speed stirring conditions are at 1080 r / min and stirring and mixing for 36 minutes; the mixed filler is a mixture of three types of alumina with a particle size ratio of 12:5:1.5 and a weight ratio of 5:3:2; the mass ratio of the mixed filler to the silane coupling agent KH560 is 15:1;
[0065] S2, heating and melting the epoxy resin, adding the mixture to stir and mix, adding acrylic acid and triphenylphosphine and heating treatment, adding modified BN and modified filler in batches and stirring and mixing to obtain a prefabricated material; wherein the heating and melting temperature is 92°C; the condition of adding in batches is to add in 4 batches in equal amounts; the condition of heating treatment is to heat to 109°C and keep warm for 1.5h; the condition of stirring and mixing is to stir and mix at 90°C for 17min; the mixture is formed by mixing hydroquinone and p-hydroxyanisole in a mass ratio of 3:2;
[0066] The mass ratio of the epoxy resin, the mixture, acrylic acid, triphenylphosphine, modified BN and modified filler is 30:0.42:10:0.39:20.8:62;
[0067] S3, adding curing agent and 2-butanone to the prefabricated material and stirring evenly, and then curing to obtain resin glue; wherein the stirring time is 2.4h;
[0068] The mass ratio of the prefabricated material, the curing agent and the solvent is 100:1.62:25; the curing agent is a mixture of 2-methylimidazole and dicyandiamide in a mass ratio of 1:3;
[0069] The preparation method of the modified BN comprises the following steps:
[0070] S11, stirring and mixing silane coupling agent KH570, ethanol and deionized water to obtain a mixed solution; wherein the mass ratio of the silane coupling agent KH570, ethanol and deionized water is 2:70:25;
[0071] S12, dispersing BN in an alkaline solution and performing ultrasonic treatment, centrifugally separating and taking out a solid, adding the solid to the mixed solution for heating reaction, centrifugally separating and taking out the solid for drying to obtain a preform; wherein the alkaline solution is a sodium hydroxide aqueous solution with a mass concentration of 12%; the mass ratio of BN to the sodium hydroxide aqueous solution is 1:9.2; the conditions of the ultrasonic treatment are 72° C. and ultrasonic treatment for 3.4 hours; the conditions of the heating reaction are 62° C. and reaction for 3 hours; the mass ratio of BN to the mixed solution is 1:1.2;
[0072] S13, mixing the preform, toluene and perhydropolysilazane, subjecting them to ultrasonic reaction, centrifuging to remove the toluene, and drying to obtain modified BN; wherein the mass ratio of the preform, toluene and perhydropolysilazane is 1.08:100:2.2; the ultrasonic reaction is carried out at 60°C for 2 hours; the drying is carried out at a microwave frequency of 2.45 GHz for 5 minutes and at 67°C for 10 hours.
[0073] Example 4
[0074] The preparation method of the resin glue comprises the following steps:
[0075] S1. After heating and drying the mixed filler, a coupling agent is added and stirred at high speed to obtain a modified filler; wherein the heating and drying conditions are at a temperature of 76°C and drying for 2.3 hours; the high-speed stirring conditions are at 1120 r / min and stirring and mixing for 39 minutes; the mixed filler is a mixture of three types of alumina with a particle size ratio of 12:5:1.5 and a weight ratio of 5:3:2; the mass ratio of the mixed filler to the silane coupling agent KH560 is 15:1;
[0076] S2, heating and melting the epoxy resin, adding the mixture to stir and mix, adding acrylic acid and triphenylphosphine and heating treatment, adding modified BN and modified filler in batches and stirring and mixing to obtain a prefabricated material; wherein the heating and melting temperature is 93°C; the condition of adding in batches is to add in equal amounts in 4 batches; the condition of heating treatment is to heat to 111°C and keep warm for 1.5h; the condition of stirring and mixing is to stir and mix at 90°C for 18min; the mixture is mixed by hydroquinone and p-hydroxyanisole in a mass ratio of 3:2;
[0077] The mass ratio of the epoxy resin, the mixture, acrylic acid, triphenylphosphine, modified BN and modified filler is 30:0.43:10:0.4:21.2:63;
[0078] S3, adding curing agent and 2-butanone to the prefabricated material and stirring evenly, and then curing to obtain resin glue; wherein the stirring time is 2.6h;
[0079] The mass ratio of the prefabricated material, the curing agent and the solvent is 100:1.68:25; the curing agent is a mixture of 2-methylimidazole and dicyandiamide in a mass ratio of 1:3;
[0080] The preparation method of the modified BN comprises the following steps:
[0081] S11, stirring and mixing silane coupling agent KH570, ethanol and deionized water to obtain a mixed solution; wherein the mass ratio of the silane coupling agent KH570, ethanol and deionized water is 2:70:25;
[0082] S12, dispersing BN in an alkaline solution and performing ultrasonic treatment, centrifugally separating and taking out a solid, adding the solid to the mixed solution for heating reaction, centrifugally separating and taking out the solid for drying to obtain a preform; wherein the alkaline solution is a sodium hydroxide aqueous solution with a mass concentration of 12%; the mass ratio of BN to the sodium hydroxide aqueous solution is 1:9.3; the conditions of the ultrasonic treatment are 73° C. and ultrasonic treatment for 3.6 hours; the conditions of the heating reaction are 63° C. and reaction for 3 hours; the mass ratio of BN to the mixed solution is 1:1.3;
[0083] S13. After mixing the preform, toluene and perhydropolysilazane, subjecting them to ultrasonic reaction, centrifuging to remove the toluene and drying to obtain modified BN; wherein the mass ratio of the preform, toluene and perhydropolysilazane is 1.12:100:2.2; the ultrasonic reaction is carried out at 60°C for 2 hours; and the drying is carried out at a microwave frequency of 2.45 GHz for 5 minutes and at 68°C for 10 hours.
[0084] Example 5
[0085] The preparation method of the resin glue comprises the following steps:
[0086] S1. After heating and drying the mixed filler, a coupling agent is added and stirred at high speed to obtain a modified filler; wherein the heating and drying conditions are at a temperature of 78°C and drying for 2.4 hours; the high-speed stirring conditions are at 1160r / min and stirring and mixing for 42 minutes; the mixed filler is a mixture of three types of alumina with a particle size ratio of 12:5:1.5 and a weight ratio of 5:3:2; the mass ratio of the mixed filler to the silane coupling agent KH560 is 15:1;
[0087] S2, heating and melting the epoxy resin, adding the mixture to stir and mix, adding acrylic acid and triphenylphosphine and heating treatment, adding modified BN and modified filler in batches and stirring and mixing to obtain a prefabricated material; wherein the heating and melting temperature is 94°C; the condition of adding in batches is to add in equal amounts in 4 batches; the condition of heating treatment is to heat to 113°C and keep warm for 1.5h; the condition of stirring and mixing is to stir and mix at 90°C for 19min; the mixture is formed by mixing hydroquinone and p-hydroxyanisole in a mass ratio of 3:2;
[0088] The mass ratio of the epoxy resin, the mixture, acrylic acid, triphenylphosphine, modified BN and modified filler is 30:0.44:10:0.41:21.6:64;
[0089] S3, adding curing agent and 2-butanone to the prefabricated material and stirring evenly, and then curing to obtain resin glue; wherein the stirring time is 2.8h;
[0090] The mass ratio of the prefabricated material, the curing agent and the solvent is 100:1.74:25; the curing agent is a mixture of 2-methylimidazole and dicyandiamide in a mass ratio of 1:3;
[0091] The preparation method of the modified BN comprises the following steps:
[0092] S11, stirring and mixing silane coupling agent KH570, ethanol and deionized water to obtain a mixed solution; wherein the mass ratio of the silane coupling agent KH570, ethanol and deionized water is 2:70:25;
[0093] S12, dispersing BN in an alkaline solution and performing ultrasonic treatment, centrifugally separating and taking out a solid, adding the solid to the mixed solution for heating reaction, centrifugally separating and taking out the solid for drying to obtain a preform; wherein the alkaline solution is a sodium hydroxide aqueous solution with a mass concentration of 12%; the mass ratio of BN to the sodium hydroxide aqueous solution is 1:9.4; the conditions of the ultrasonic treatment are 74° C. and ultrasonic treatment for 3.7 hours; the conditions of the heating reaction are 64° C. and reaction for 3 hours; the mass ratio of BN to the mixed solution is 1:1.4;
[0094] S13. After mixing the preform, toluene and perhydropolysilazane, subjecting them to ultrasonic reaction, centrifuging to remove the toluene and drying to obtain modified BN; wherein the mass ratio of the preform, toluene and perhydropolysilazane is 1.16:100:2.2; the ultrasonic reaction conditions are 60°C for 2h; the drying conditions are 2.45GHz microwave frequency, 5min treatment, 69°C for 10h drying.
[0095] Example 6
[0096] The preparation method of the resin glue comprises the following steps:
[0097] S1. After heating and drying the mixed filler, a coupling agent is added and stirred at high speed to obtain a modified filler; wherein the heating and drying conditions are at 80°C and drying for 2.5 hours; the high-speed stirring conditions are at 1200r / min and stirring and mixing for 45 minutes; the mixed filler is a mixture of three types of alumina with a particle size ratio of 12:5:1.5 and a weight ratio of 5:3:2; the mass ratio of the mixed filler to the silane coupling agent KH560 is 15:1;
[0098] S2, heating and melting the epoxy resin, adding the mixture to stir and mix, adding acrylic acid and triphenylphosphine and heating treatment, adding modified BN and modified filler in batches and stirring and mixing to obtain a prefabricated material; wherein the heating and melting temperature is 95°C; the condition of adding in batches is to add in 4 batches in equal amounts; the condition of heating treatment is to heat to 115°C and keep warm for 1.5h; the condition of stirring and mixing is to stir and mix at 90°C for 20min; the mixture is formed by mixing hydroquinone and p-hydroxyanisole in a mass ratio of 3:2;
[0099] The mass ratio of the epoxy resin, the mixture, acrylic acid, triphenylphosphine, modified BN and modified filler is 30:0.45:10:0.42:22:65;
[0100] S3, adding curing agent and 2-butanone to the prefabricated material and stirring evenly, and then curing to obtain resin glue; wherein the stirring time is 3 hours;
[0101] The mass ratio of the prefabricated material, the curing agent and the solvent is 100:1.8:25; the curing agent is a mixture of 2-methylimidazole and dicyandiamide in a mass ratio of 1:3;
[0102] The preparation method of the modified BN comprises the following steps:
[0103] S11, stirring and mixing silane coupling agent KH570, ethanol and deionized water to obtain a mixed solution; wherein the mass ratio of the silane coupling agent KH570, ethanol and deionized water is 2:70:25;
[0104] S12, dispersing BN in an alkaline solution and performing ultrasonic treatment, centrifugally separating and taking out a solid, adding the solid to the mixed solution for heating reaction, centrifugally separating and taking out the solid for drying to obtain a preform; wherein the alkaline solution is a sodium hydroxide aqueous solution with a mass concentration of 12%; the mass ratio of BN to the sodium hydroxide aqueous solution is 1:9.5; the conditions of the ultrasonic treatment are 75°C and ultrasonic treatment for 3.8 hours; the conditions of the heating reaction are 65°C and reaction for 3 hours; the mass ratio of BN to the mixed solution is 1:1.5;
[0105] S13. After mixing the preform, toluene and perhydropolysilazane, subjecting them to ultrasonic reaction, centrifuging to remove the toluene and drying to obtain modified BN; wherein the mass ratio of the preform, toluene and perhydropolysilazane is 1.2:100:2.2; the ultrasonic reaction is carried out at 60°C for 2 hours; and the drying is carried out at a microwave frequency of 2.45 GHz for 5 minutes and at 70°C for 10 hours.
[0106] Comparative Example 1
[0107] Compared with Example 4, the difference is that the mixed filler of Comparative Example 1 is a mixture of two types of aluminum oxide with a particle size ratio of 5:1.5 and a weight ratio of 3:2; the other components, preparation steps and parameters are the same.
[0108] Comparative Example 2
[0109] Compared with Example 4, the difference is that the mixed filler of Comparative Example 2 is a mixture of two types of aluminum oxide with a particle size ratio of 12:1.5 and a weight ratio of 5:2; the other components, preparation steps and parameters are the same.
[0110] Comparative Example 3
[0111] Compared with Example 4, the difference is that the mixed filler of Comparative Example 3 is a mixture of two types of aluminum oxide with a particle size ratio of 12:5 and a weight ratio of 5:3; the other components, preparation steps and parameters are the same.
[0112] Comparative Example 4
[0113] Compared with Example 4, the difference is that the mixed filler of Comparative Example 4 is a mixture of three types of aluminum oxide with a particle size ratio of 9:5:1.5 and a weight ratio of 4:3:2; the other components, preparation steps and parameters are the same.
[0114] Comparative Example 5
[0115] Compared with Example 4, the difference is that acrylic acid is not added in Comparative Example 5; the other components, preparation steps and parameters are the same.
[0116] Comparative Examples 6-7
[0117] Compared with Example 4, the difference is that the mixture of Comparative Example 6-7 is prepared by mixing hydroquinone and p-hydroxyanisole in a mass ratio of 3:2; the other components, preparation steps and parameters are the same.
[0118] Table 1 (Unit: parts by weight)
[0119] Hydroquinone p-Hydroxyanisole Example 4 3 2 Comparative Example 6 0 5 Comparative Example 7 5 0
[0120] Comparative Example 8
[0121] Compared with Example 4, the difference is that Comparative Example 8 uses BN instead of modified BN; the other components, preparation steps and parameters are the same.
[0122] Comparative Example 9
[0123] Compared with Example 4, the difference is that Comparative Example 9 does not use perhydropolysilazane; the remaining components, preparation steps and parameters are the same.
[0124] Comparative Example 10
[0125] Compared with Example 4, the difference is that the drying conditions of step S13 of Comparative Example 10 are at a temperature of 68° C. and drying for 10 hours.
[0126] The resin adhesives prepared in Examples 1-6 and Comparative Examples 1-10 were subjected to thermal conductivity test (ASTM D5470-2006, the test method is steady-state heat flow method) and peel strength test (IPC-TM-6502.4.8). The test results are shown in Table 2.
[0127] Table 2
[0128]
[0129]
[0130] From the test results in Table 2, it can be seen that compared with Comparative Examples 1-10, the thermal conductivity and peel strength of the resin adhesive of the second embodiment of the present invention are significantly better than those of Comparative Examples 1-10.
[0131] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A packaging process for a mobile storage device, characterized in that: The packaging process comprises the following steps: 1) Preliminarily fix the controller, electrical components and memory chips on the substrate by using resin glue; 2) Solder the controller, electrical components, memory chip and substrate with solder paste; 3) Solder gold wires between the memory chip, controller, electrical components and the upper surface of the substrate, and perform reflow soldering to obtain a semi-finished product; 4) Check the welding condition of semi-finished products, and conduct H2 test on the semi-finished products after welding; 5) After the H2 test is completed, the shell is assembled, the outer surface of the shell is laser engraved, and then it is packaged to complete the processing; The preparation method of the resin glue comprises the following steps: S1. After heating and drying the mixed filler, adding a coupling agent and stirring at high speed to obtain a modified filler; wherein the mixed filler is a mixture of three fillers with a particle size ratio of 12:5:1.5 and a weight ratio of 5:3:2; the filler is alumina; the heating and drying conditions are at a temperature of 70-80°C and drying for 2-2.5 hours; the high-speed stirring conditions are at 1000-1200r / min and stirring and mixing for 30-45min; the mass ratio of the mixed filler to the coupling agent is 15:1; the coupling agent is one or both of a silane coupling agent and a titanate coupling agent; S2, heating and melting the epoxy resin, adding the mixture and stirring and mixing, adding acrylic acid and a catalyst and heating treatment, adding modified BN and a modified filler in batches and stirring and mixing to obtain a prefabricated material; wherein the mixture is formed by mixing hydroquinone and p-hydroxyanisole in a mass ratio of 3:2; the temperature of the heating and melting is 90-95°C; the condition of the batch addition is to add equal amounts in 4 batches; the condition of the heating treatment is to heat to 105-115°C and keep warm for 1.5h; the condition of stirring and mixing is to stir and mix at 90°C for 15-20min; the catalyst is triphenylphosphine; the mass ratio of the epoxy resin, the mixture, acrylic acid, the catalyst, the modified BN and the modified filler is 30:0.40-0.45:10:0.37-0.42:20-22:60-65; S3, adding curing agent and solvent to the prefabricated material, stirring evenly, and curing to obtain resin glue; Wherein, the preparation method of the modified BN comprises the following steps: S11, stirring and mixing the silane coupling agent, ethanol and deionized water to obtain a mixed solution; S12, dispersing BN in an alkaline solution and subjecting it to ultrasonic treatment, centrifuging to obtain a solid, adding it to the mixed solution for heating reaction, centrifuging to obtain a solid, and drying it to obtain a preform; S13, mixing the preform, toluene and perhydropolysilazane, subjecting the mixture to ultrasonic reaction, removing the toluene by centrifugation, and drying to obtain modified BN.
2. The packaging process of a mobile storage device according to claim 1, characterized in that: The parameters of the laser engraving are a laser wavelength of 400-3500nm, a power of 5-12W, a frequency of 0.1-220KHz, a laser routing speed of 0.01-50000mm / s, and a filling spacing of 0.01-6mm.
3. The packaging process of a mobile storage device according to claim 1, characterized in that: The surface of the substrate contains a metal film layer, and the metal film layer contains one or more of Cu element, Ni element, Zn element and Ti element.
4. The packaging process of a mobile storage device according to claim 1, characterized in that: In step S3, the uniform stirring time is 2-3 hours; the mass ratio of the prefabricated material, the curing agent and the solvent is 100:1.5-1.8:25; the curing agent is a mixture of 2-methylimidazole and dicyandiamide in a mass ratio of 1:3; and the solvent is 2-butanone.
5. The packaging process of a mobile storage device according to claim 1, characterized in that: In step S11, the silane coupling agent is silane coupling agent KH570; the mass ratio of the silane coupling agent, ethanol and deionized water is 2:70:25; in step S12, the alkaline solution is a sodium hydroxide aqueous solution with a mass concentration of 12%; the mass ratio of BN to the sodium hydroxide aqueous solution is 1:9.0-9.5; the conditions of the ultrasonic treatment are 70-75°C and ultrasound for 3.2-3.8h; the conditions of the heating reaction are 60-65°C and reaction for 3h; the mass ratio of BN to the mixed solution is 1:1.0-1.
5.
6. The packaging process of a mobile storage device according to claim 1, characterized in that: In step S13, the mass ratio of the preform, toluene and perhydropolysilazane is 1.0-1.2:100:2.2; the ultrasonic reaction is carried out at 60°C for 2 hours; and the drying is carried out at a microwave frequency of 2.45 GHz for 5 minutes and at 65-70°C for 10 hours.