Aqueous zinc ion half-cell electrolyte, full-cell electrolyte, and aqueous zinc ion battery

By adding N-benzyloxycarbonyl-L-threonine to the electrolyte of zinc ion battery, the dendrite and corrosion problems in zinc ion battery are solved, the cycle life and stability of the battery are improved, and the energy storage field is promoted. Application.

CN117638259BActive Publication Date: 2024-11-22NEW MATERIAL INST OF SHANDONG ACADEMY OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311643578.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-04
Publication Date
2024-11-22
Estimated Expiration
2043-12-04

AI Technical Summary

Technical Problem

Zinc ion batteries are prone to form zinc dendrites during circulation, resulting in accelerated hydrogen precipitation, local pH changes and by-product generation, which in turn affects the deposition/peeling efficiency of zinc negative electrodes, limiting its commercialization and wide application.

Method used

Add N-benzyloxycarbonyl-L-threonine to the electrolyte to regulate the deposition direction of zinc ions, avoid dendrites, and reduce water molecules contact by adsorption on the surface of zinc metal anode to alleviate corrosion reactions.

Benefits of technology

Significantly reduce the corrosion and by-product generation of zinc metal anodes, improve the cycle life and stability of zinc ion batteries, and promote its application in the field of large-scale energy storage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004585185460000011
    Figure HDA0004585185460000011
  • Figure HDA0004585185460000012
    Figure HDA0004585185460000012
  • Figure HDA0004585185460000021
    Figure HDA0004585185460000021
Patent Text Reader

Abstract

The present invention provides an aqueous zinc ion half-cell electrolyte, a full-cell electrolyte, and an aqueous zinc ion battery, and belongs to the field of battery technology. The electrolyte provided by the present invention comprises deionized water, an electrolyte and an additive, and the additive is N-benzyloxycarbonyl-L-threonine. The present invention uses N-benzyloxycarbonyl-L-threonine as an additive, and its strong affinity to the surface of the zinc metal anode induces zinc ions to deposit on the (002) crystal plane, refines the grains, and forms a fine-grained zinc deposition layer. And it has a stronger adsorption effect on the crystal plane, isolating the direct contact between free water and the zinc anode surface, thereby reducing the hydrogen evolution reaction on the zinc anode surface, effectively avoiding the formation of zinc dendrites, and can also significantly reduce the corrosion and by-product generation on the surface of the zinc metal anode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to an aqueous zinc ion half-cell electrolyte, a full-cell electrolyte, and an aqueous zinc ion battery. Background Art

[0002] The development of battery energy storage systems is one of the hot topics in the current energy field. In particular, lithium-ion batteries have dominated the consumer electronics market since their introduction due to their high energy density, excellent cycle performance, and good multi-scenario compatibility. However, serious problems such as high cost, leakage of toxic substances, and potential for combustion and explosion have gradually been exposed in the development of lithium-ion batteries and have been criticized. Therefore, the development of efficient and available alternative products is what people expect.

[0003] Compared with traditional lithium-ion batteries based on organic electrolytes, aqueous zinc-ion batteries (ZIBs) have attracted much attention due to their unique advantages, such as high theoretical capacity, low redox potential (-0.76V relative to the standard hydrogen electrode), high safety, high abundance, simple preparation conditions and environmental protection. However, zinc dendrites are easily formed at the zinc negative electrode during the cycle of zinc-ion batteries. The formation of dendrites accelerates the rate of hydrogen evolution in aqueous batteries, and the accelerated hydrogen evolution leads to changes in local pH, thereby forming byproducts. The accumulation of ZHS on the surface of the zinc negative electrode exacerbates the surface unevenness and increases the polarization. The increased polarization will intensify the growth of zinc dendrites. Therefore, problems such as dendrite problems, hydrogen evolution problems and side reactions affect and intensify each other. This vicious cycle leads to extremely low efficiency of zinc negative electrode deposition / stripping, which is not conducive to its commercialization and widespread application.

[0004] Among them, electrolyte additives have the most significant effect in inhibiting the growth of zinc dendrites, and trace amounts of additives do not require too much process cost. Therefore, it is of great significance to find a low-cost, non-toxic, and abundant additive to optimize the zinc ion battery electrolyte, thereby improving the zinc negative electrode and enhancing the electrochemical stability and cycle life of aqueous zinc ion batteries. Summary of the invention

[0005] In view of this, the object of the present invention is to provide an aqueous zinc ion half-cell electrolyte, a full-cell electrolyte, and an aqueous zinc ion battery. The present invention alleviates the hydrogen evolution corrosion reaction of the zinc metal anode in the aqueous zinc ion battery by adding N-benzyloxycarbonyl-L-threonine to the electrolyte, thereby significantly reducing the corrosion on the surface of the zinc metal anode and the generation of by-products.

[0006] In order to achieve the above-mentioned object, the present invention provides the following technical solution: an aqueous zinc ion half-cell electrolyte, comprising deionized water, an electrolyte and an additive; the additive is N-benzyloxycarbonyl-L-threonine.

[0007] In some embodiments, in the aqueous zinc ion half-cell electrolyte, the concentration of N-benzyloxycarbonyl-L-threonine is 0.001 mol / L to 0.04 mol / L, preferably 0.02 mol / L to 0.035 mol / L, and more preferably 0.03 mol / L.

[0008] In some embodiments, the electrolyte is zinc sulfate heptahydrate.

[0009] In some embodiments, the concentration of zinc sulfate is 0.5 mol / L to 2 mol / L, preferably 1 mol / L.

[0010] The present invention also provides an aqueous zinc ion full-battery electrolyte, comprising deionized water, an electrolyte and an additive; the electrolyte is zinc sulfate heptahydrate and manganese sulfate monohydrate; and the additive is N-benzyloxycarbonyl-L-threonine.

[0011] In some embodiments, in the aqueous zinc ion full battery electrolyte, the concentration of the N-benzyloxycarbonyl-L-threonine is 0.001 mol / L to 0.04 mol / L, preferably 0.02 mol / L to 0.035 mol / L, and more preferably 0.03 mol / L, the concentration of the zinc sulfate is 0.5 mol / L to 2 mol / L, preferably 1 mol / L, and the concentration of the manganese sulfate monohydrate is 0.01 mol / L to 0.3 mol / L, and preferably 0.2 mol / L.

[0012] The present invention also provides an aqueous zinc ion battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the electrolyte is the electrolyte described in any one of the above technical solutions.

[0013] In some embodiments, the active material of the positive electrode is MnO2, the material of the negative electrode is high-purity zinc metal, and the separator is glass fiber.

[0014] In some embodiments, the preparation method of MnO2 is a hydrothermal synthesis. Specifically, 5 mmol K2MnO4 is first dissolved in 70 mL H20 and slowly stirred clockwise with a glass rod. After it is dissolved, 1.75 mL of concentrated HCl is added. After stirring at room temperature for 30 minutes, it is transferred to a reactor and heated in a drying oven at 100°C for 6 hours.

[0015] In some embodiments, when the positive electrode active material is MnO2, the preparation method of the positive electrode sheet is: firstly grind MnO2 and the conductive agent in a mortar respectively, then mix MnO2, the conductive agent and the binder in a mass ratio of 7:2:1, use N-methylpyrrolidone as a solvent, grind them evenly in a mortar, and evenly apply the ground slurry on a PE film with a 200um scraper in a coating infrared dryer, and then put it in a vacuum drying box for drying, and after drying, use a cutting machine to cut it into a positive electrode sheet with a diameter of 12mm. In the present invention, the conductive agent is preferably Ketjen black, and the binder is preferably PVDF.

[0016] In some embodiments, the negative electrode material further comprises zinc sheet, zinc foil, or zinc alloy.

[0017] Beneficial technical effects:

[0018] 1. The present invention uses N-benzyloxycarbonyl-L-threonine as an additive for aqueous zinc ion battery electrolyte, and uses ZnSO4 as a basic electrolyte. In the process of zinc deposition, N-benzyloxycarbonyl-L-threonine induces zinc ions to deposit in the direction of the (002) crystal plane, which has the effect of refining grains and regulating the uniform deposition of zinc ions. In addition, since zinc atoms mainly grow horizontally on the (002) crystal plane of the zinc metal anode, the formation of dendrites can be effectively avoided. In addition, since N-benzyloxycarbonyl-L-threonine is more easily adsorbed on the surface of the zinc metal anode and has a larger adsorption energy on the (002) crystal plane, it can hinder the direct contact between water molecules and the zinc metal anode, reduce the water content at the interface between the zinc metal anode and the electrolyte, thereby alleviating the hydrogen evolution corrosion reaction of the zinc metal anode, and can significantly reduce the corrosion on the surface of the zinc metal anode and the generation of by-products.

[0019] 2. The N-benzyloxycarbonyl-L-threonine additive added to the electrolyte of the present invention has the effect of inhibiting dendrite growth and hydrogen evolution corrosion, which can significantly improve the cycle life and stability of aqueous zinc ion batteries, and is of great significance in promoting its application in the field of large-scale energy storage. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The figures are contact angle test graphs of the electrolytes prepared in Example 1 and Comparative Example 1, wherein Figure (a) is a contact angle test graph of the electrolyte obtained in Example 1, and Figure (b) is a contact angle test graph of the electrolyte obtained in Comparative Example 1;

[0021] Figure 2The SEM images of the zinc electrode in the Zn / / Zn symmetrical battery assembled with the electrolytes prepared in Example 1 and Comparative Example 1 after 100 cycles of deposition in the electrolyte at a magnification of 2000 times, wherein Figure (a) is a SEM image of the zinc electrode in the Zn / / Zn symmetrical battery assembled with the electrolyte prepared in Example 1 after 100 cycles of deposition in the electrolyte at a magnification of 2000 times, and Figure (b) is a SEM image of the zinc electrode in the Zn / / Zn symmetrical battery assembled with the electrolyte prepared in Comparative Example 1 after 100 cycles of deposition in the electrolyte at a magnification of 2000 times;

[0022] Figure 3 This is a test diagram of the cycle life of a Zn / / Zn symmetrical battery assembled with the electrolytes prepared in Example 1 and Comparative Example 1;

[0023] Figure 4 The rate performance diagram of the Zn / / Zn symmetric battery assembled with the electrolytes prepared in Example 1 and Comparative Example 1;

[0024] Figure 5 The Tafel curve of an aqueous zinc ion three-electrode battery assembled with the electrolytes prepared in Example 1 and Comparative Example 1;

[0025] Figure 6 Long cycle performance diagram of aqueous zinc ion battery Zn / / MnO2 assembled with electrolytes prepared in Example 2 and Comparative Example 2;

[0026] Figure 7 The rate performance diagram of aqueous zinc ion battery Zn / / MnO2 assembled with the electrolyte prepared in Example 2 and Comparative Example 2;

[0027] Figure 8 This is a linear voltammetric scan test diagram of an aqueous zinc ion battery Zn / / MnO2 assembled with the electrolytes prepared in Example 2 and Comparative Example 2. DETAILED DESCRIPTION

[0028] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.

[0029] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.

[0030] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0031] Example 1

[0032] Preparation of aqueous zinc ion half-cell electrolyte:

[0033] Dissolve 28.756g of zinc sulfate heptahydrate in 50mL of deionized water, stir until completely dissolved, and then use a 100mL volumetric flask to make a 100mL electrolyte for standby use. Take out 10mL of the electrolyte, add 0.0759g of N-benzyloxycarbonyl-L-threonine thereto, and ultrasonically disperse it at room temperature until the N-benzyloxycarbonyl-L-threonine is completely dissolved, and then let it stand to obtain an aqueous zinc ion half-cell electrolyte containing N-benzyloxycarbonyl-L-threonine.

[0034] The contact angle of the aqueous zinc ion half-cell electrolyte prepared in Example 1 was tested using a contact angle measuring instrument. Figure 1 As shown in (a), the contact angle is 79°.

[0035] Comparative Example 1

[0036] Preparation of 1M ZnSO4 electrolyte without additives:

[0037] Dissolve 28.756 g of zinc sulfate heptahydrate in 50 mL of deionized water, stir it with a magnetic stirrer to completely dissolve it, and then use a 100 mL volumetric flask to make up to 100 mL of electrolyte.

[0038] The contact angle of the aqueous zinc ion electrolyte without additives prepared in Comparative Example 1 was tested using a contact angle measuring instrument. The contact angle was as follows: Figure 1 As shown in (b), the contact angle is 96°, which is larger than the contact angle of 79° measured in Example 1. The results show that the aqueous zinc ion electrolyte containing N-benzyloxycarbonyl-L-threonine has a greater adsorption energy on the zinc foil. In the battery, N-benzyloxycarbonyl-L-threonine is more easily adsorbed on the surface of the zinc foil than water molecules, which can hinder the direct contact between water molecules and the zinc metal anode, reduce the water content at the interface between the zinc metal anode and the electrolyte, and thus alleviate the hydrogen evolution corrosion reaction of the zinc metal anode.

[0039] Test Example 1

[0040] The electrolyte prepared in Example 1 was used to assemble a Zn / / Zn symmetrical battery and tested on a blue light test system. Figure 2 (a) Zn / / Zn symmetric cell at a current density of 1 mA / cm 2 , deposition capacity is 1 mAh / cm 2 SEM image after 100 cycles under the test conditions. Figure 2 From the SEM image in (a), it can be observed that after 100 cycles of the Zn / / Zn symmetric battery, the surface of the zinc anode is very flat and uniform, indicating that the zinc deposition is uniform and dense, and no zinc dendrites and by-products are generated.

[0041] The electrolyte prepared in Example 1 was used to assemble a Zn / / Zn symmetrical battery, and a charge and discharge test was performed on a blue-power test system. Figure 3 As shown, at a current density of 1 mA / cm 2 , deposition capacity is 1 mAh / cm 2 Under the test conditions, the cycle life of the Zn / / Zn symmetric battery can exceed 2000h and exhibits a stable polarization voltage.

[0042] The additive-free aqueous zinc ion electrolyte prepared in Comparative Example 1 was used to assemble a Zn / / Zn symmetrical battery, and a charge and discharge test was performed on a blue power test system. Figure 3 As shown, at a current density of 1 mA / cm 2 , deposition capacity is 1 mAh / cm 2 Under the test conditions, the Zn / / Zn symmetrical battery short-circuited at around 200 hours, and the voltage polarization was very unstable. It may be that zinc dendrites were generated inside the battery, which pierced the diaphragm and caused the battery to short-circuit.

[0043] Figure 4 The rate performance diagram of the Zn / / Zn symmetric battery assembled with the electrolytes prepared in Example 1 and Comparative Example 1 shows that the overall performance of the Zn / / Zn symmetric battery containing N-benzyloxycarbonyl-L-threonine is stable, while the Zn / / Zn symmetric battery without N-benzyloxycarbonyl-L-threonine short-circuits when cycled for more than 60 times, and the voltage polarization is very unstable.

[0044] Figure 5 The Tafel curves of the aqueous zinc ion three-electrode battery in Example 1 and Comparative Example 1 show that the corrosion current of the three-electrode battery containing N-benzyloxycarbonyl-L-threonine is 2.364×10 -3 mA / cm 2 , which is much smaller than the corrosion current of the three-electrode battery without N-benzyloxycarbonyl-L-threonine, which is 5.557×10 -3 mA / cm 2 This proves that N-benzyloxycarbonyl-L-threonine additive can slow down the corrosion of aqueous zinc ion electrolyte on battery electrodes.

[0045] Example 2

[0046] Preparation of aqueous zinc ion full battery electrolyte: Same as Example 1, except that 0.2 mol of MnSO4 is also added to the electrolyte.

[0047] Comparative Example 2

[0048] The same as comparative example 1, except that 0.2 mol of MnSO4 is also added to the electrolyte.

[0049] Test Example 2

[0050] The electrolytes prepared in Example 2 and Comparative Example 2 were used to assemble Zn / / MnO2 full batteries, and the long cycle performance test was carried out on a blue power test system. Figure 6 As shown, at a current density of 1 mA / cm 2 , deposition capacity is 1 mAh / cm 2 Under the test conditions, compared with the full battery of Comparative Example 2, the capacity decay of the aqueous zinc ion battery using the electrolyte of Example 2 is slower, and it has higher coulombic efficiency and cycle stability.

[0051] Figure 7 The rate performance diagram of the aqueous zinc ion battery Zn / / MnO2 full cell assembled with the electrolytes prepared in Example 2 and Comparative Example 2 shows that the discharge specific capacity of the Zn / / MnO2 full cell containing N-benzyloxycarbonyl-L-threonine at current densities of 1A / g, 2A / g, 3A / g, 4A / g, 5A / g and 1A / g is significantly higher than that of the Zn / / MnO2 full cell not containing N-benzyloxycarbonyl-L-threonine, indicating that the aqueous zinc-manganese battery with the new electrolyte based on N-benzyloxycarbonyl-L-threonine as the electrolyte additive has better rate performance.

[0052] Figure 8 The linear voltammetric scan test diagram of the aqueous zinc ion battery Zn / / MnO2 full cell assembled with the electrolytes prepared in Example 2 and Comparative Example 2. It can be seen from the figure that at a scan rate of 0.1 mV / s, the Zn / / MnO2 full cell containing N-benzyloxycarbonyl-L-threonine and the Zn / / MnO2 full cell not containing N-benzyloxycarbonyl-L-threonine both have two oxidation peaks and two reduction peaks, and the positions of the oxidation peaks and the reduction peaks almost completely overlap, indicating that N-benzyloxycarbonyl-L-threonine does not change the chemical reaction of the positive electrode active material.

[0053] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. An aqueous zinc ion half-cell electrolyte, characterized in that The invention comprises deionized water, electrolyte and additive; the additive is N-benzyloxycarbonyl-L-threonine; In the aqueous zinc ion half-cell electrolyte, the concentration of N-benzyloxycarbonyl-L-threonine is 0.001 mol / L to 0.04 mol / L; The electrolyte is zinc sulfate heptahydrate; In the aqueous zinc ion half-cell electrolyte, the concentration of zinc sulfate is 0.5 mol / L to 2 mol / L.

2. An aqueous zinc ion full battery electrolyte, characterized in that: It comprises deionized water, electrolyte and additive; the electrolyte is zinc sulfate heptahydrate and manganese sulfate monohydrate; the additive is N-benzyloxycarbonyl-L-threonine; In the aqueous zinc ion full battery electrolyte, the concentration of N-benzyloxycarbonyl-L-threonine is 0.001 mol / L to 0.04 mol / L, the concentration of zinc sulfate is 0.5 mol / L to 2 mol / L, and the concentration of manganese sulfate monohydrate is 0.01 mol / L to 0.3 mol / L.

3. An aqueous zinc ion battery, characterized in that: It comprises a positive electrode, a negative electrode, a separator and an electrolyte, wherein the electrolyte is the electrolyte according to claim 1 or 2; the active material of the positive electrode is MnO2, the material of the negative electrode is high-purity zinc metal, and the separator is glass fiber.