An antibacterial card protection film and its preparation process

By using a combination of a modified hot melt adhesive layer and a hydrophobic crosslinking layer in the card protection film and performing dynamic irradiation of ultraviolet rays, the problem of insufficient moisture-proof and antibacterial performance of the card protection film in humid environments is solved, and the card protection film is realized The excellent performance of the membrane in harsh environments.

CN117644707BActive Publication Date: 2024-11-08HUIZHOU YIDU STATIONERY SUPPLIES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311560396.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-22
Publication Date
2024-11-08
Estimated Expiration
2043-11-22

AI Technical Summary

Technical Problem

The existing card protection film is difficult to maintain moisture-proof and antibacterial properties in humid and harsh environments, resulting in problems such as moisture in data, mold corrosion and blurred handwriting.

Method used

Using a modified hot melt adhesive layer composed of ethylene-vinyl acetate copolymer, cetyl trimethyl ammonium bromide, caprolactam, 4-phenyl benzophenone and aqueous acrylic resin, combined with silane coupling agent, The hydrophobic crosslinking layer prepared by isopropanol and alcohol-soluble polyurethane is crosslinked by dynamic irradiation of ultraviolet rays to form an antibacterial protective film.

Benefits of technology

The card protection film maintains excellent moisture-proof and antibacterial properties in a long-term humid environment, ensuring that the data is dry and not moldy, and the preparation process is simple and easy to control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004562237570000121
    Figure BDA0004562237570000121
  • Figure BDA0004562237570000131
    Figure BDA0004562237570000131
Patent Text Reader

Abstract

The present application provides an antibacterial card protection film, comprising a substrate layer, an intermediate layer, a modified hot melt adhesive layer and a hydrophobic cross-linking layer; wherein the modified hot melt adhesive layer is prepared by cross-linking and modification of ethylene-vinyl acetate copolymer, hexadecyltrimethylammonium bromide, caprolactam, 4-phenylbenzophenone and an aqueous acrylic resin; by modifying the ethylene-vinyl acetate copolymer material of the hot melt adhesive layer and covering its surface with a hydrophobic cross-linking layer, a silane coupling agent and isopropyl alcohol fall into the active sites of the modified ethylene-vinyl acetate copolymer layer, so that the entire antibacterial card protection film has more excellent hydrophobicity and antibacterial properties, and even if it is in a humid environment for a long time, the material protected by the card protection film can still be kept dry and moldy, with a better effect and convenient for promotion and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of card protection film preparation, and in particular to an antibacterial card protection film and a preparation process thereof. Background Art

[0002] Card protection film, also known as plastic sealing film, has the advantages of being moisture-proof, dust-proof and anti-fading. It is a commonly used tool for protecting documents and photos.

[0003] The card protection film is composed of a polyester film layer, a polyethylene film layer and an EVA vinyl acetate copolymer film layer from the inside to the outside.

[0004] At present, card protection films are usually used to store photos, credit cards and various certificates in daily life. The storage environment is relatively clean and dry, and card protection films can fully play a good protective role. However, for special environments, such as damp, dark and moldy environments, when various materials exist, especially for long-term storage, conventional card protection films are difficult to guarantee excellent moisture-proof and antibacterial properties, and the materials may become damp, mold corrosion and blurred handwriting, which brings great challenges to the storage of important materials in harsh special environments.

[0005] Therefore, it is of great significance to develop a card protection film that can be stored for a long time in a humid and harsh environment and has excellent moisture-proof and antibacterial properties. Summary of the invention

[0006] The purpose of the present invention is to provide an antibacterial card protection film and its preparation process in view of the problem that the existing card protection film has poor moisture-proof and antibacterial effects after being placed in a humid environment for a long time. The card protection film provided by the present application has excellent moisture-proof and antibacterial properties. Even if it is placed in a humid environment for a long time, it can still ensure that the materials protected by the card protection film are dry and not moldy, and the effect is better.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is:

[0008] An antibacterial card protection film comprises a substrate layer, an intermediate layer, a modified hot melt adhesive layer and a hydrophobic cross-linking layer.

[0009] Furthermore, the raw materials of the modified hot melt adhesive layer include the following materials:

[0010] 30-50 parts by weight of ethylene-vinyl acetate copolymer, 5-15 parts by weight of cetyltrimethylammonium bromide, 3-8 parts by weight of caprolactam, 3-8 parts by weight of 4-phenylbenzophenone, and 5-10 parts by weight of water-based acrylic resin;

[0011] Furthermore, the raw materials of the hydrophobic cross-linking layer include the following materials:

[0012] 10-20 parts by weight of silane coupling agent, 20-40 parts by weight of isopropyl alcohol, and 8-15 parts by weight of alcohol-soluble polyurethane.

[0013] Furthermore, the raw materials of the modified hot melt adhesive layer include the following materials:

[0014] 40-50 parts by weight of ethylene-vinyl acetate copolymer;

[0015] 8-15 parts by weight of hexadecyltrimethylammonium bromide;

[0016] 5-8 parts by weight of caprolactam;

[0017] 5 to 8 parts by weight of 4-phenylbenzophenone;

[0018] 5 to 8 parts by weight of water-based acrylic resin.

[0019] Furthermore, the hydrophobic cross-linked layer is mainly made of the following materials:

[0020] 12 to 18 parts by weight of silane coupling agent;

[0021] 30-40 parts by weight of isopropyl alcohol;

[0022] 10 to 15 parts by weight of alcohol-soluble polyurethane.

[0023] The study found that the weight ratio of each raw material is the key factor affecting the moisture resistance and antibacterial properties of the card protection film. Only through the selection of raw material types and the coordination of the ratios can excellent comprehensive performance be demonstrated.

[0024] Furthermore, the substrate layer is a BOPET polyester substrate layer, and the middle layer is a polyethylene film layer.

[0025] Furthermore, when the card protection film is used, the substrate layer faces inward, close to the object to be protected, and the hydrophobic cross-linking layer is the outermost layer, which is used to directly contact the environment.

[0026] Furthermore, one part by weight of the raw material of the modified hot melt adhesive layer is consistent with one part by weight of the raw material of the hydrophobic cross-linking layer.

[0027] Another object of the present invention is to provide a method for preparing the antibacterial card protection film.

[0028] The preparation process of the antibacterial card protection film comprises the following steps:

[0029] Step 1, compounding the substrate layer and the intermediate layer;

[0030] Step 2, flowing the melt of the modified hot melt adhesive onto the middle layer, and obtaining a modified hot melt adhesive layer after cooling;

[0031] Step 3, then contacting and soaking the raw material mixture of the modified hot melt adhesive layer and the hydrophobic cross-linking layer for 1.5 hours to 3 hours, and then taking out;

[0032] Step 4: Then, the modified hot melt adhesive layer after soaking is irradiated with ultraviolet rays to obtain the card protection film.

[0033] Furthermore, the step 2 also includes stretching, calendering and composite trimming with a cooling roller; wherein the temperature of the cooling roller is below 50°C; preferably, the temperature of the cooling roller is 25°C to 50°C.

[0034] Furthermore, the modified hot melt adhesive is mainly prepared by the following method:

[0035] First, ethylene-vinyl acetate copolymer and water-based acrylic resin are mixed and heated to 60° C. to 80° C. to obtain a premix;

[0036] Then, caprolactam and 4-phenylbenzophenone are added to the premix, and the mixture is heated to 120° C. to 150° C. under stirring conditions and maintained for 1 h to 2 h. Then, hexadecyltrimethylammonium bromide is added thereto under heat preservation conditions, and the mixture is rapidly stirred and cooled to obtain a modified hot melt adhesive.

[0037] Furthermore, the rapid stirring rate is 300 to 500 rpm; and the rapid stirring time is 20 to 40 min.

[0038] Furthermore, the raw material mixture of the hydrophobic cross-linking layer is mainly prepared by the following method:

[0039] According to the raw material ratio, silane coupling agent KH570, alcohol-soluble polyurethane and isopropyl alcohol are mixed, and the temperature is slowly raised to 60° C. to 90° C. while stirring, and then quickly cooled to 25° C. to 35° C. within 5 min to 10 min to obtain a raw material mixture for a hydrophobic cross-linking layer.

[0040] Furthermore, during the mixing process of the raw materials for the hydrophobic cross-linking layer, the stirring rate is 80 to 150 revolutions per minute; and the temperature is raised to 60° C. to 90° C. within 40 to 60 minutes.

[0041] Furthermore, it is characterized in that the specific method of ultraviolet irradiation is as follows:

[0042] Step S1, irradiate with a UV lamp with a power of 12W or more for 5min to 10min;

[0043] Step S2, irradiating with an ultraviolet lamp with a power of less than 8W for 5min to 10min;

[0044] Step S3, repeating steps S1 and S2 until the total irradiation and cross-linking time reaches 2h to 4h, and the irradiation is completed.

[0045] The study found that the use of dynamic cross-irradiation of high and low power UV lamps can better retain the adhesion of the hydrophobic cross-linked layer. Compared with static UV lamp irradiation, the overall performance of the product is more outstanding.

[0046] Furthermore, in step S1, an ultraviolet lamp with a power of 12w to 15w is used for irradiation.

[0047] Furthermore, in step S2, an ultraviolet lamp with a power of 6w to 8w is used for irradiation.

[0048] Furthermore, the substrate layer is a BOPET polyester substrate layer, and the middle layer is a polyethylene film layer.

[0049] Furthermore, the preparation method of the BOPET polyester substrate layer is: biaxially stretching the polyester sheet in the longitudinal and transverse directions and cutting the polyester sheet to form the BOPET polyester substrate layer.

[0050] Furthermore, the polyester sheet is obtained by casting PET resin.

[0051] Furthermore, the method for preparing the polyethylene film layer is as follows: the polyethylene melt is flowed onto the substrate layer, and then the polyethylene film layer is prepared by stretching, calendering, and compound trimming using a cooling roller.

[0052] The present application provides a method for preparing a card protection film. Compared with the traditional preparation method, the preparation process adds the steps of immersion to form a hydrophobic cross-linking layer and dynamic irradiation curing with ultraviolet light. The entire preparation process is simple to operate and easy to control. The formed card protection film exhibits outstanding moisture resistance and antibacterial properties.

[0053] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0054] 1. The present invention cross-links hydrophobic substances and antibacterial substances on the modified hot-melt adhesive layer, so that it has a strong hydrophobic antibacterial effect, and then the surface is attached with a hydrophobic cross-linking layer prepared by silane coupling agent, isopropyl alcohol and alcohol-soluble polyurethane. The silane coupling agent and isopropyl alcohol fall into the active sites of the modified hot-melt adhesive layer, so that the entire antibacterial card protection film has more excellent hydrophobicity and antibacterial properties. Even if it is in a humid environment for a long time, it can still ensure that the material protected by the card protection film is dry and moldy, the effect is better, and it is easy to promote and apply.

[0055] 2. The present invention provides a method for preparing a card protection film. Compared with the traditional preparation method, the preparation process adds the steps of immersion to form a hydrophobic cross-linking layer and dynamic irradiation curing with ultraviolet light. The whole preparation process is simple to operate and easy to control. The formed card protection film exhibits outstanding moisture resistance and antibacterial properties. DETAILED DESCRIPTION

[0056] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0057] Example 1

[0058] Preparation of modified hot melt adhesive

[0059] Prepare materials: 40 parts by weight of ethylene-vinyl acetate copolymer; 8 parts by weight of cetyltrimethylammonium bromide; 5 parts by weight of caprolactam; 5 parts by weight of 4-phenylbenzophenone; and 8 parts by weight of water-based acrylic resin.

[0060] First, ethylene-vinyl acetate copolymer and water-based acrylic resin are mixed and heated to 70° C. to obtain a premix;

[0061] Then, caprolactam and 4-phenylbenzophenone were added to the premix, and the mixture was heated to 130° C. under stirring and maintained for 1.5 hours. Then, hexadecyltrimethylammonium bromide was added thereto under heat preservation conditions, and rapid stirring was performed at a rate of 400 rpm and a rapid stirring time of 30 minutes. The mixture was cooled to obtain a modified hot melt adhesive.

[0062] Preparation of hydrophobic cross-linking layer raw material mixture

[0063] Prepare materials: 18 parts by weight of silane coupling agent KH570; 30 parts by weight of isopropyl alcohol; 10 parts by weight of alcohol-soluble polyurethane.

[0064] According to the raw material ratio, silane coupling agent KH570, alcohol-soluble polyurethane and isopropanol were mixed, stirred (stirring rate was 120 rpm), heated to 80° C. within 50 min, and then quickly cooled to 30° C. within 8 min to obtain a raw material mixture for a hydrophobic cross-linking layer.

[0065] Preparation of card protection film

[0066] Step 1, biaxially stretching and cutting the polyester sheet to form a BOPET polyester substrate layer;

[0067] Step 2, flowing the polyethylene melt onto the BOPET polyester substrate layer obtained in step 1, and performing stretching, calendering, composite trimming using a cooling roller to prepare a polyethylene film layer;

[0068] Step 3, flowing the melt of the modified hot melt adhesive onto the polyethylene film layer obtained in step 2, and performing stretching, calendering, composite trimming by using a cooling roller (30° C.) to prepare a modified hot melt adhesive layer;

[0069] Step 4, then immersing the modified hot melt adhesive layer prepared in step 3 in the raw material mixture of the hydrophobic cross-linking layer for 2 hours, and then taking it out;

[0070] Step 5: Then, facing one side of the modified hot melt adhesive layer soaked in the composite material layer, a UV lamp is used for dynamic irradiation cross-linking to prepare a card protection film;

[0071] Among them, the specific method of dynamic irradiation cross-linking by ultraviolet lamp is as follows:

[0072] Step S1, irradiation with a UV lamp of 13W for 8min;

[0073] Step S2, irradiate with an ultraviolet lamp with a power of 8W for 8 minutes;

[0074] Step S3, repeating steps S1 and S2 until the total irradiation and cross-linking time reaches 3 hours, and the irradiation is completed.

[0075] The formed card protection film includes a BOPET polyester base material layer, a polyethylene film layer, a modified hot melt adhesive layer and a hydrophobic cross-linking layer which are laid sequentially from the inside to the outside.

[0076] Example 2

[0077] Preparation of modified hot melt adhesive

[0078] Prepare the following materials: 50 parts by weight of ethylene-vinyl acetate copolymer; 15 parts by weight of hexadecyltrimethylammonium bromide; 8 parts by weight of caprolactam; 8 parts by weight of 4-phenylbenzophenone; and 8 parts by weight of water-based acrylic resin.

[0079] First, ethylene-vinyl acetate copolymer and water-based acrylic resin are mixed and heated to 80° C. to obtain a premix;

[0080] Then, caprolactam and 4-phenylbenzophenone were added to the premix, and the mixture was heated to 150° C. under stirring and maintained for 2 hours. Then, hexadecyltrimethylammonium bromide was added thereto under heat preservation conditions, and rapid stirring was performed at a rate of 500 rpm and a rapid stirring time of 40 minutes. The mixture was cooled to obtain a modified hot melt adhesive.

[0081] Preparation of hydrophobic cross-linking layer raw material mixture

[0082] Prepare materials: 12 parts by weight of silane coupling agent KH570; 40 parts by weight of isopropyl alcohol; 15 parts by weight of alcohol-soluble polyurethane.

[0083] According to the raw material ratio, silane coupling agent KH570, alcohol-soluble polyurethane and isopropanol are mixed, stirred (stirring rate is 150 rpm), heated to 90°C within 60 minutes, and then quickly cooled to 25°C to 35°C within 10 minutes to obtain a raw material mixture for a hydrophobic cross-linking layer.

[0084] Preparation of card protection film

[0085] Step 1, biaxially stretching and cutting the polyester sheet to form a BOPET polyester substrate layer;

[0086] Step 2, flowing the polyethylene melt onto the BOPET polyester substrate layer obtained in step 1, and performing stretching, calendering, composite trimming using a cooling roller to prepare a polyethylene film layer;

[0087] Step 3, flowing the melt of the modified hot melt adhesive onto the polyethylene film layer in the first composite material layer obtained in step 2, and performing stretching, calendering, composite trimming by using a cooling roller (50° C.) to prepare a modified hot melt adhesive layer;

[0088] Step 4, then immersing the modified hot melt adhesive layer prepared in step 3 in the raw material of the hydrophobic cross-linking layer for 3 hours, and then taking it out;

[0089] Step 5: Then, facing one side of the modified hot melt adhesive layer soaked in the composite material layer, a UV lamp is used for dynamic irradiation cross-linking to prepare a card protection film;

[0090] Among them, the specific method of dynamic irradiation cross-linking by ultraviolet lamp is as follows:

[0091] Step S1, irradiate with a 15W UV lamp for 5 minutes;

[0092] Step S2, irradiate with an ultraviolet lamp with a power of 8W for 5 minutes;

[0093] Step S3, repeating steps S1 and S2 until the total irradiation and cross-linking time reaches 2 hours, and the irradiation is completed.

[0094] The formed card protection film includes a BOPET polyester base material layer, a polyethylene film layer, a modified hot melt adhesive layer and a hydrophobic cross-linking layer which are laid sequentially from the inside to the outside.

[0095] Example 3

[0096] Preparation of modified hot melt adhesive layer

[0097] Prepare materials: 30 parts by weight of ethylene-vinyl acetate copolymer; 5 parts by weight of cetyltrimethylammonium bromide; 3 parts by weight of caprolactam; 3 parts by weight of 4-phenylbenzophenone; and 5 parts by weight of water-based acrylic resin.

[0098] First, ethylene-vinyl acetate copolymer and water-based acrylic resin are mixed and heated to 60° C. to obtain a premix;

[0099] Then, caprolactam and 4-phenylbenzophenone were added to the premix, and the mixture was heated to 120° C. under stirring and maintained for 2 hours. Then, hexadecyltrimethylammonium bromide was added thereto under heat preservation conditions, and rapid stirring was performed at a rate of 300 rpm and a rapid stirring time of 40 minutes to obtain a modified hot melt adhesive.

[0100] Preparation of hydrophobic cross-linking layer raw material mixture

[0101] Prepare materials: 10 parts by weight of silane coupling agent KH570; 20 parts by weight of isopropyl alcohol; 8 parts by weight of alcohol-soluble polyurethane.

[0102] According to the raw material ratio, silane coupling agent KH570, alcohol-soluble polyurethane and isopropanol were mixed, stirred (stirring rate was 80 rpm), heated to 60° C. within 40 min, and then quickly cooled to 25° C. within 10 min to obtain a raw material mixture for a hydrophobic cross-linking layer.

[0103] Preparation of card protection film

[0104] Step 1, biaxially stretching and cutting the polyester sheet to form a BOPET polyester substrate layer;

[0105] Step 2, flowing the polyethylene melt onto the BOPET polyester substrate layer obtained in step 1, and performing stretching, calendering, composite trimming using a cooling roller to prepare a polyethylene film layer;

[0106] Step 3, flowing the raw material melt of the modified hot melt adhesive layer onto the polyethylene film layer obtained in step 2, and performing stretching, calendering, composite trimming by using a cooling roller (25° C.) to prepare a modified hot melt adhesive layer;

[0107] Step 4, then soaking the modified hot melt adhesive layer prepared in step 3 in the raw material of the hydrophobic cross-linking layer for 1.5 hours, and then taking it out;

[0108] Step 5: Then, facing one side of the modified hot melt adhesive layer soaked in the composite material layer, a UV lamp is used for dynamic irradiation cross-linking to prepare a card protection film;

[0109] Among them, the specific method of dynamic irradiation cross-linking by ultraviolet lamp is as follows:

[0110] Step S1, irradiate with a 12W UV lamp for 10 min;

[0111] Step S2, irradiate with a 6W ultraviolet lamp for 10 min;

[0112] Step S3, repeating steps S1 and S2 until the total irradiation and cross-linking time reaches 4 hours, and the irradiation is completed.

[0113] The formed card protection film includes a BOPET polyester base material layer, a polyethylene film layer, a modified hot melt adhesive layer and a hydrophobic cross-linking layer which are laid sequentially from the inside to the outside.

[0114] Comparative Example 1

[0115] The card protection film provided in Comparative Example 1 is different in that the hot melt adhesive layer is not modified, the raw material is only ethylene-vinyl acetate copolymer, and no hydrophobic cross-linking layer is provided, and the rest is exactly the same as Example 1. The formed card protection film includes a BOPET polyester substrate layer, a polyethylene film layer, and an ethylene-vinyl acetate copolymer layer laid sequentially from the inside to the outside.

[0116] Comparative Example 2

[0117] The difference between Comparative Example 2 and Example 1 is that no hydrophobic cross-linking layer is provided, and the rest is completely the same as Example 1. The formed card protection film includes a BOPET polyester substrate layer, a polyethylene film layer and a modified hot melt adhesive layer which are sequentially laid from the inside to the outside.

[0118] Comparative Example 3

[0119] Comparative Example 3 is different from Example 1 in that the hot melt adhesive layer is not modified, the raw material is only ethylene-vinyl acetate copolymer, and the rest is exactly the same as Example 1. The formed card protection film includes a BOPET polyester substrate layer, a polyethylene film layer, an ethylene-vinyl acetate copolymer layer and a hydrophobic cross-linking layer laid sequentially from the inside to the outside.

[0120] Comparative Example 4

[0121] The difference between Comparative Example 4 and Example 1 is that the ultraviolet irradiation adopts static irradiation, and the other aspects are exactly the same as Example 1.

[0122] The specific method of static irradiation cross-linking by UV lamp is as follows:

[0123] The side of the modified hot melt adhesive layer soaked in the composite material layer was statically irradiated with a 13W ultraviolet lamp for 3 hours to prepare a card protection film.

[0124] Comparative Example 5

[0125] The difference between Comparative Example 5 and Example 1 is that the ultraviolet irradiation adopts static irradiation, and the other aspects are exactly the same as Example 1.

[0126] The specific method of static irradiation cross-linking by UV lamp is as follows:

[0127] The side of the modified hot melt adhesive layer soaked in the composite material layer was statically irradiated with an ultraviolet lamp with a power of 8W for 3 hours to prepare a card protection film.

[0128] Test 1

[0129] According to GB / T 1037-1988 standard, the water vapor permeability coefficients of the card protection film materials of Examples 1 to 3 and Comparative Examples 1 to 5 were tested respectively by a water vapor tester (the water vapor permeability coefficient is the ratio of the water vapor permeability of the obtained card protection film material to that of the BOPET polyester substrate layer, expressed in percentage %, and the lower the water vapor permeability coefficient, the better the hydrophobic performance and the better the water barrier property of the material). The test results are shown in Table 1.

[0130] Test 2

[0131] The antibacterial effects of the card protection film materials prepared in Examples 1-3 and Comparative Examples 1-5 were tested respectively with reference to the step of Section 5 Bacterial Barrier in Wet Conditions of YY / T0471.5 Test Method for Contact Wound Surgery Film. The tested bacteria were Aspergillus niger, and the test results are shown in Table 1.

[0132] Test 3

[0133] A4 paper with handwriting that is easily blurred when exposed to water was placed in the card protection films prepared in Examples 1-3 and Comparative Examples 1-5 for sealing, and then the sealed documents were placed in a sealing device that can maintain high humidity (relative humidity reaches 95%) and high mold content. After 6 months, all the sealed documents were taken out, the card protection film was opened, and the status of the A4 paper was recorded. The recording results are shown in Table 1.

[0134] Table 1 Test results of hydrophobicity and antibacterial properties of card protection film

[0135]

[0136]

[0137] Therefore, it can be seen from the test results in Table 1 that the modification of ethylene-vinyl acetate copolymer and the arrangement of the hydrophobic cross-linking layer are the key factors for the card protection film to maintain excellent hydrophobicity and antibacterial properties. Even if it is in a humid environment for a long time, it can still ensure that the material protected by the card protection film is dry and moldy, with better effect.

[0138] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An antibacterial card protection film, characterized in that: It includes a substrate layer, an intermediate layer, a modified hot melt adhesive layer and a hydrophobic cross-linking layer; the raw materials of the hydrophobic cross-linking layer include the following materials: 10 to 20 parts by weight of silane coupling agent, 20 to 40 parts by weight of isopropyl alcohol, and 8 to 15 parts by weight of alcohol-soluble polyurethane; the substrate layer is a BOPET polyester substrate layer; the intermediate layer is a polyethylene film layer; the raw materials of the modified hot melt adhesive layer include the following materials: 40 to 50 parts by weight of ethylene-vinyl acetate copolymer, 8 to 15 parts by weight of hexadecyltrimethylammonium bromide, 5 to 8 parts by weight of caprolactam, 5 to 8 parts by weight of 4-phenylbenzophenone, and 5 to 8 parts by weight of water-based acrylic resin; The method for preparing the card protection film comprises the following steps: Step 1, compounding the substrate layer and the intermediate layer; Step 2, flowing the melt of the modified hot melt adhesive onto the middle layer, and obtaining a modified hot melt adhesive layer after cooling; Step 3, then contacting and soaking the raw material mixture of the modified hot melt adhesive layer and the hydrophobic cross-linking layer for 1.5 hours to 3 hours, and then taking out; Step 4, then irradiating the soaked modified hot melt adhesive layer with ultraviolet light to obtain the card protection film; The specific method of ultraviolet irradiation in step 4 is as follows: Step S1, irradiate with a UV lamp with a power of 12W or more for 5min to 10min; Step S2, irradiating with an ultraviolet lamp with a power of less than 8W for 5min to 10min; Step S3, repeating steps S1 and S2 until the total irradiation and cross-linking time reaches 2h to 4h, and the irradiation is completed.

2. The card protection film according to claim 1, characterized in that: The hydrophobic cross-linking layer is mainly prepared from the following materials: 12 to 18 parts by weight of a silane coupling agent, 30 to 40 parts by weight of isopropyl alcohol, and 10 to 15 parts by weight of an alcohol-soluble polyurethane.

3. A method for preparing a card protection film according to any one of claims 1 to 2, characterized in that: The following steps are involved: Step 1, compounding the substrate layer and the intermediate layer; Step 2, flowing the melt of the modified hot melt adhesive onto the middle layer, and obtaining a modified hot melt adhesive layer after cooling; Step 3, then contacting and soaking the raw material mixture of the modified hot melt adhesive layer and the hydrophobic cross-linking layer for 1.5 hours to 3 hours, and then taking out; Step 4, then irradiating the soaked modified hot melt adhesive layer with ultraviolet light to obtain the card protection film; The specific method of ultraviolet irradiation in step 4 is as follows: Step S1, irradiate with a UV lamp with a power of 12W or more for 5min to 10min; Step S2, irradiating with an ultraviolet lamp with a power of less than 8W for 5min to 10min; Step S3, repeating steps S1 and S2 until the total irradiation and cross-linking time reaches 2h to 4h, and the irradiation is completed.

4. The preparation method according to claim 3, characterized in that: The modified hot melt adhesive in step 2 is mainly prepared by the following method: First, ethylene-vinyl acetate copolymer and water-based acrylic resin are mixed and heated to 60° C. to 80° C. to obtain a premix; Then, caprolactam and 4-phenylbenzophenone are added to the premix, and the mixture is heated to 120° C. to 150° C. under stirring conditions and maintained for 1 h to 2 h. Then, hexadecyltrimethylammonium bromide is added thereto under heat preservation conditions, and the mixture is rapidly stirred and cooled to obtain a modified hot melt adhesive.

5. The preparation method according to claim 4, characterized in that: The rapid stirring rate is 300 to 500 rpm; the rapid stirring time is 20 to 40 min.

6. The preparation method according to claim 4, characterized in that: The raw material mixture of the hydrophobic cross-linking layer is mainly prepared by the following method: according to the raw material ratio, silane coupling agent KH570, alcohol-soluble polyurethane and isopropyl alcohol are mixed, and the temperature is slowly raised to 60° C. to 90° C. while stirring, and then quickly cooled to 25° C. to 35° C. within 5 min to 10 min to obtain the raw material mixture of the hydrophobic cross-linking layer.

7. The preparation method according to claim 6, characterized in that: The stirring rate is 80 to 150 rpm; the slow heating refers to heating to 60° C. to 90° C. within 40 to 60 minutes.