A multi-component composite stabilized zirconium oxide thermal barrier coating material and preparation method thereof
By doping tetravalent B elements and trivalent rare earth oxides in the zirconia thermal barrier coating, combined with plasma spraying and flame spraying technology, a multi-component composite zirconia with low thermal conductivity, high temperature phase stability and long thermal cycle life is prepared. The coating solves the problem of existing coatings falling off at high temperatures and is suitable for thermal insulation protection of high-temperature components.
Patent Information
- Application Number
- CN202311642427.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-01
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-12-01
AI Technical Summary
Existing zirconia thermal barrier coatings are prone to problems such as tetragonal to monoclinic phase transformation and sintering at temperatures above 1200°C, resulting in coating peeling and failure, and cannot meet higher temperature service requirements.
The multi-component stable zirconia thermal barrier coating material is used, including doped tetravalent B elements and trivalent rare earth oxides, with the chemical formula (Zr1-xBx)O2-yA2O3. It is prepared by atmospheric plasma spraying process, combined with supersonic flame spraying of metal Bonding layer, forming a coating with low thermal conductivity, high temperature phase stability and long thermal cycle life.
It achieves the effects of low thermal conductivity, high bonding strength, good thermal insulation performance and long thermal cycle life. It is suitable for large-scale mass production and suitable for thermal insulation protection of high-temperature components such as gas turbines and aerospace engines.
Smart Images

Figure CN117658629B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high-temperature thermal barrier materials, and in particular to a multi-component composite stable zirconia thermal barrier coating material and a preparation method thereof. Background Art
[0002] The turbine inlet temperature of heavy-duty gas turbines is high, reaching over 1400°C. The gas temperature of advanced military gas turbines even reaches 1500°C-1800°C. Such extremely high temperatures make the operating environment of the hot-end components of gas turbines very harsh. Nickel-based high-temperature alloys, which are commonly used as substrates for high-temperature components, have a temperature tolerance limit of only about 1100°C, which cannot meet the application requirements of existing gas turbines or aircraft engines. Thermal barrier coatings (TBCs) are composite coatings composed of a metal bonding layer and a ceramic layer with good heat resistance and thermal insulation. It mainly reduces the surface temperature of the heated parts by isolating the heated substrate from the high-temperature medium. Its preparation method is not limited by the shape of the hot-end components and has almost no effect on the mechanical properties of the substrate material. Therefore, the preparation of thermal barrier coatings on the surface of high-temperature components is the preferred economical and effective way to increase the temperature tolerance of components.
[0003] Thermal barrier coating materials require the following: high melting point, high temperature phase stability, low thermal conductivity, high chemical stability, high thermal expansion coefficient, sintering resistance, etc. Zirconia ceramics have the advantages of relatively low thermal conductivity, high melting point and high thermal expansion coefficient, so they are used as the preferred material for thermal barrier ceramic layers. However, pure zirconium oxide has three crystal structures. The crystal structure changes at different temperatures, resulting in volume changes and large internal stresses, which cause cracks in the coating material and lead to failure. Studies have found that yttria partially stabilized zirconia (6% to 8% YSZ) has good thermal cycling, high melting point, low thermal conductivity and other properties, and is considered to be the most ideal ceramic layer material at present. However, when the temperature is higher than 1200°C, the YSZ coating is prone to problems such as tetragonal phase to monoclinic phase transformation and sintering, which leads to coating shedding and failure, and cannot meet the service requirements of higher temperatures. Therefore, it is urgent to research and develop a new type of high-performance zirconia thermal barrier ceramic coating material to further reduce thermal conductivity, improve phase stability and sintering resistance, and extend service life to meet the higher temperature service requirements of gas turbine hot end components. Therefore, a multi-component composite stable zirconia thermal barrier coating material is needed. Summary of the invention
[0004] The purpose of the present invention is to provide a multi-component composite stable zirconia thermal barrier coating material having the advantages of low thermal conductivity, high temperature phase stability, long thermal cycle life and the like.
[0005] To achieve the above object, the present invention is implemented according to the following technical solutions:
[0006] The thermal barrier coating material of the present invention comprises a tetravalent B element and a trivalent rare earth oxide, and the chemical formula of the thermal barrier coating material is (Zr 1-x B x )O2-yA2O3, 2. wherein x is the content of doped tetravalent B element, y is the mass percentage of doped trivalent rare earth oxide, wherein 0.1≤x≤0.3, 10≤y≤25, and the particle size of the thermal barrier coating material is 25 to 75 μm.
[0007] Furthermore, the tetravalent B element oxide BO2 is any two or more of TiO2, HfO2, CeO2, and MoO2.
[0008] Furthermore, the trivalent rare earth oxide A2O3 is any four or more of Gd2O3, Yb2O3, Nd2O3, Pr2O3, Sm2O3, Er2O3, and Dy2O3.
[0009] In another aspect, a multi-component composite stabilized zirconia thermal barrier coating comprises a metal bonding layer and a thermal barrier ceramic layer, wherein the thermal barrier ceramic layer comprises a tetravalent B element and a trivalent rare earth oxide, and the chemical formula of the thermal barrier ceramic layer is (Zr 1-x B x )O2-yA2O3, 2. wherein x is the content of doped tetravalent B element, y is the mass percentage of doped trivalent rare earth oxide, that is, the mass percentage of trivalent rare earth oxide is y%, wherein 0.1≤x≤0.3, 10≤y≤25, the metal bonding layer comprises one or more of CoNi CrAlY, NiCoCrAlY or NiCoCrAl TaY, the thickness of the metal bonding layer is 100-200 μm, the metal bonding adopts supersonic flame spraying to prepare the metal bonding layer on the alloy substrate; and atmospheric plasma spraying is adopted to prepare the surface thermal barrier ceramic layer on the surface of the metal bonding layer.
[0010] Furthermore, the atmospheric plasma spraying process parameters are: argon flow rate is 35-45L / min, hydrogen flow rate is 8-15L / min, nitrogen flow rate is 15-25L / min; current is 500-650A, working voltage is 60-80V, spraying distance is 110-150mm, spray gun moving speed is 650-1000mm / min, powder feeding speed is 30-50g / min. The thickness of the surface thermal barrier zirconia ceramic layer is 300-1000μm.
[0011] In another aspect, a method for preparing a multi-component composite stabilized zirconia thermal barrier coating material comprises the following steps:
[0012] 1) four or more rare earth oxides A2O3, two or more tetravalent metal oxides BO2 and ZrOCl2·8H2O are weighed in a stoichiometric ratio of (0.1-0.3):(10-25), and the oxides are dissolved in diluted concentrated nitric acid or concentrated sulfuric acid, and ZrOCl2·8H2O is dissolved in deionized water;
[0013] 2) mixing the two solutions, adding polyethylene glycol dispersant, and stirring with a glass rod to obtain a clear mixed solution;
[0014] 3) Under ultrasonic vibration environment, reversely titrate the mixed solution into an ammonia solution to form a colloidal precipitate, maintain the pH value of the ammonia solution ≥ 10 during the titration process, and let it stand for 24 hours after the titration is completed;
[0015] 4) centrifuging and washing the colloidal precipitate with deionized water at a centrifugal speed of 5000-8000 r / min until the pH value of the supernatant after centrifugation is neutral, washing it with anhydrous ethanol, and drying it in an oven to obtain a precursor powder;
[0016] 5) sintering the precursor powder in an air environment at 1200° C. to 1400° C. for 5 to 8 hours to obtain a composite rare earth stabilized zirconia thermal barrier ceramic material;
[0017] 6) wet-milling the composite rare earth stabilized zirconia thermal barrier ceramic material to obtain a slurry, wherein the ball milling medium is anhydrous ethanol and the ball milling beads are made of zirconia;
[0018] 7) placing the slurry in a drying oven for drying to obtain powder, the drying temperature is 80-100° C., and the drying time is 15-20 hours;
[0019] 8) adding the dried powder to a ball mill for mixing to obtain a mixed slurry;
[0020] 9) subjecting the mixed slurry to centrifugal spray granulation to obtain agglomerated powder;
[0021] 10) Sintering, crushing and screening the agglomerated powder to obtain the multi-component composite stable zirconia thermal barrier ceramic material spray powder.
[0022] Furthermore, in step (6), the ball milling speed is 400-600 r / min, and the ball milling time is 20-30 h.
[0023] Furthermore, in step (8), the rotation speed of the ball mill is 300 to 500 r / min, and the ball mill mixing time is 15 to 25 h.
[0024] Furthermore, in step (8), 15 to 30 wt.% of deionized water, 3 to 6 wt.% of polyacrylic acid and 2 to 5 wt.% of polyvinyl alcohol are added.
[0025] Furthermore, in the centrifugal spray granulation in step (9), the centrifugal speed is 15000-20000 rpm, the air inlet temperature is 250-320° C., the air outlet temperature is 100-150° C., and the feed rate is 30-45 rpm.
[0026] Furthermore, in step (10), the sintering temperature is 1200-1400° C., and the sintering holding time is 2-6 hours.
[0027] The beneficial effects of the present invention are:
[0028] Compared with the prior art, the present invention has the following technical effects:
[0029] The composite rare earth stabilized zirconia thermal barrier coating material of the present invention has the advantages of low thermal conductivity, high bonding strength, good thermal insulation performance, long thermal cycle life, etc., and the material preparation process is reliable, the performance is stable, and it is suitable for large-scale batch production. It has a good promotion prospect in the field of thermal insulation protection of hot end components such as gas turbines and aircraft engines. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is the XRD curve of the multi-component composite stabilized zirconia thermal barrier ceramic material prepared in Example 1 and Example 3 of the present invention.
[0031] Figure 2 This is a SEM picture of the multi-component composite stabilized zirconia thermal barrier ceramic material powder prepared in Example 1 of the present invention;
[0032] Figure 3 This is a SEM picture of the multi-component composite stabilized zirconia thermal barrier ceramic material powder prepared in Example 3 of the present invention; DETAILED DESCRIPTION
[0033] The present invention is further described below with specific examples. The illustrative examples and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.
[0034] like Figure 1 As shown, Example 1:
[0035] (Zr 0.85 Ce 0.1 T i 0.05 )O2-5.2Gd2O3-5.6Yb2O3-4.8Nd2O3-4.5Pr2O3 thermal barrier ceramic material and spraying powder, comprising the following steps:
[0036] 1) According to the stoichiometric ratio, TiO2 (purity 99.99%), CeO2 (purity 99.99%), Gd2O3 (purity 99.99%), Yb2O3 (purity 99.99%), Nd2O3 (99.99%), and Pr2O3 (99.99%) are weighed and dissolved in diluted concentrated nitric acid and mixed and stirred until clear; according to the stoichiometric ratio, ZrOCl2·8H2O powder is weighed and dissolved in deionized water and stirred;
[0037] 2) mixing the two clear solutions, adding polyethylene glycol dispersant, and stirring with a glass rod to obtain a clear mixed solution;
[0038] 3) Under ultrasonic vibration environment, reverse titrate the mixed solution into the ammonia solution to form a colloidal precipitate. During the titration process, the pH value of the ammonia solution is maintained at ≥10. After the titration is completed, let it stand for 24 hours;
[0039] 4) The colloidal precipitate is centrifuged and washed with deionized water at a centrifugal speed of 5000-8000 r / min until the pH value of the supernatant after centrifugation is neutral, and then washed with anhydrous ethanol and dried in an oven to obtain a precursor powder;
[0040] 5) The colloidal precipitate is centrifuged and washed with deionized water at a centrifugal speed of 8000 r / min until the pH value of the supernatant after centrifugation is neutral, and then washed with anhydrous ethanol and dried in an oven at 80° C. to obtain a precursor powder;
[0041] 6) The precursor powder was heated to 1200°C at a heating rate of 5°C and sintered for 6 hours to obtain (Zr 0.85 Ce 0.1 T i 0.05 )O2-5.2Gd2O3-5.6Yb2O3-4.8Nd2O3-4.5Pr2O3 thermal barrier ceramic materials.
[0042] 7) Prepared (Zr 0.85 Ce 0.1 T i 0.05 )O2-5.2Gd2O3-5.6Yb2O3-4.8Nd2O3-4.5Pr2O3 materials were wet ball milled, the ball milling medium was anhydrous ethanol, the ball milling beads were made of zirconia, the ball milling speed was 450r / min, and the ball milling time was 24h.
[0043] 8) The slurry obtained by ball milling is placed in a drying oven for drying at a drying temperature of 180°C and a drying time of 15 hours.
[0044] 9) Add 15 wt.% of deionized water, 4 wt.% of polyacrylic acid and 3 wt.% of polyvinyl alcohol to the dried powder and place in a ball mill for mixing. The speed of the ball mill is 400 r / min and the ball mill mixing time is 20 h.
[0045] 10) The obtained mixed slurry is subjected to centrifugal spray granulation to obtain agglomerated powder. The centrifugal speed during centrifugal spray granulation is 18000 rpm, the air inlet temperature is 300°C, the air outlet temperature is 100°C, and the feed rate is 32 rpm.
[0046] 11) The agglomerated powder is sintered at a sintering temperature of 1400°C and a sintering holding time of 3 hours. Then, the (Zr 0.85 Ce 0.1 T i 0.05 )O2-5.2Gd2O3-5.6Yb2O3-4.8Nd2O3-4.5Pr2O3 spray powder, the powder particle size is 25~75μm.
[0047] Example 2
[0048] A (Zr 0.85 Ce 0.1 T i 0.05 )O2-5.2Gd2O3-5.6Yb2O3-4.8Nd2O3-4.5Pr2O3 thermal barrier coating, comprising a metal bonding layer and a thermal barrier ceramic layer.
[0049] The Ni23Co17Cr12A10.5Y metal bonding layer was sprayed on the GH4145 nickel-based high-temperature alloy plate by supersonic flame spraying (HVOF), and the coating thickness was 100 μm.
[0050] The atmospheric plasma spraying was used to prepare the surface of the metal bonding layer (Zr 0.85 Ce 0.1 T i 0.05 )O2-5.2Gd2O3-5.6Yb2O3-4.8Nd2O3-4.5Pr2O3 surface thermal barrier ceramic layer, atmospheric plasma spraying process parameters are: argon flow rate is 40L / min, hydrogen flow rate is 10L / min, nitrogen flow rate is 15L / min; current is 580A, working voltage is 72V, spraying distance is 120mm, spray gun moving speed is 800mm / min, powder feeding speed is 40g / min, thermal barrier zirconia ceramic layer thickness is 500μm,
[0051] Embodiment 3:
[0052] A low thermal conductivity and long life composite rare earth stabilized zirconia thermal barrier ceramic material, (Zr 0.89 Hf 0.06T i 005 )-4.9La2O3-4.5Sm2O3-5.3Er2O3-5.2Dy2O3, comprising the following steps:
[0053] 1) according to the stoichiometric ratio, HfO2 (purity 99.99%), TiO2 (purity 99.99%), La2O3 (purity 99.99%), Nd2O3 (purity 99.99%), Sm2O3 (purity 99.99%), Er2O3 (99.99%), and Dy2O3 (99.99%) are weighed and dissolved in concentrated sulfuric acid and mixed and stirred until clear; according to the stoichiometric ratio, ZrOCl2·8H2O powder is weighed and dissolved in deionized water and stirred;
[0054] 2) mixing the two clear solutions, adding polyethylene glycol dispersant, and stirring with a glass rod to obtain a clear mixed solution;
[0055] 3) Under ultrasonic vibration environment, reverse titrate the mixed solution into the ammonia solution to form a colloidal precipitate. During the titration process, the pH value of the ammonia solution is maintained at ≥10. After the titration is completed, let it stand for 24 hours;
[0056] 4) The colloidal precipitate is centrifuged and washed with deionized water at a centrifugal speed of 5000-8000 r / min until the pH value of the supernatant after centrifugation is neutral, and then washed with anhydrous ethanol and dried in an oven to obtain a precursor powder;
[0057] 5) The colloidal precipitate is centrifuged and washed with deionized water at a centrifugal speed of 8000 r / min until the pH value of the supernatant after centrifugation is neutral, and then washed with anhydrous ethanol and dried in an oven at 80° C. to obtain a precursor powder;
[0058] 6) The precursor powder was heated to 1200°C at a heating rate of 5°C and sintered for 6 hours to obtain (Zr 0.89 Hf 0.06 T i 005 )-4.9La2O3-4.5Sm2O3-5.3Er2O3-5.2Dy2O3 composite rare earth stabilized zirconia thermal barrier ceramic material.
[0059] 7) Prepare (Zr 0.89 Hf 0.06 T i 005 )-4.9La2O3-4.5Sm2O3-5.3Er2O3-5.2Dy2O3 materials were wet ball milled, the ball milling medium was anhydrous ethanol, the ball milling beads were made of zirconia, the ball milling speed was 450r / min, and the ball milling time was 24h.
[0060] 8) The slurry obtained by ball milling is placed in a drying oven for drying at a drying temperature of 180°C and a drying time of 15 hours.
[0061] 9) Add 15 wt.% of deionized water, 4 wt.% of polyacrylic acid and 3 wt.% of polyvinyl alcohol to the dried powder and place in a ball mill for mixing. The speed of the ball mill is 400 r / min and the ball mill mixing time is 20 h.
[0062] 10) The obtained mixed slurry is subjected to centrifugal spray granulation to obtain agglomerated powder. The centrifugal speed during centrifugal spray granulation is 18000 rpm, the air inlet temperature is 300°C, the air outlet temperature is 100°C, and the feed rate is 32 rpm.
[0063] 11) The agglomerated powder is sintered at a sintering temperature of 1400°C and a sintering holding time of 3 hours. Then, the (Zr 0.89 Hf 0.06 T i 005 )-4.9La2O3-4.5Sm2O3-5.3Er2O3-5.2Dy2O3 spray powder, the powder particle size is 25~75μm.
[0064] Embodiment 4:
[0065] A (Zr 0.89 Hf 0.06 T i 005 )-4.9La2O3-4.5Sm2O3-5.3Er2O3-5.2Dy2O3 thermal barrier coating, comprising a metal bonding layer and a thermal barrier ceramic layer.
[0066] The Ni23Co17Cr12A10.5Y metal bonding layer was sprayed on the GH4145 nickel-based high-temperature alloy plate by supersonic flame spraying (HVOF), and the coating thickness was 100 μm.
[0067] The atmospheric plasma spraying was used to prepare the surface of the metal bonding layer (Zr 0.89 Hf 0.06 T i 005 )-4.9La2O3-4.5Sm2O3-5.3Er2O3-5.2Dy2O3 surface thermal barrier ceramic layer, atmospheric plasma spraying process parameters are: argon flow rate is 40L / min, hydrogen flow rate is 10L / min, nitrogen flow rate is 15L / min; current is 580A, working voltage is 75V, spraying distance is 120mm, spray gun moving speed is 850mm / min, powder feeding speed is 42g / min, thermal barrier zirconia ceramic layer thickness is 500μm,
[0068] Comparative Example 1:
[0069] The thermal conductivity and thermal expansion coefficient of commercially available ZrO2-8Y2O3 rare earth stabilized zirconia ceramic powder material were tested.
[0070] Comparative Example 2:
[0071] The ZrO2-8Y2O3 rare earth stabilized zirconia ceramic powder of Example 1 was used, and the method of Example 2 was used to prepare a 500 μm thick ZrO2-8Y2O3 rare earth stabilized zirconia thermal barrier ceramic coating.
[0072] Comparative Example 3:
[0073] The difference from Example 1 is that the method of Example 1 is used to prepare a two-element rare earth oxide stabilized zirconium oxide material: ZrO2-4.8% Nd2O3-4.5% Pr2O3 ceramic material and spray powder;
[0074] Comparative Example 4:
[0075] The difference from Example 2 is that the method of Example 2 is used to prepare a two-element rare earth oxide stabilized zirconium oxide coating: ZrO2-4.8% Nd2O3-4.5% Pr2O3 ceramic coating;
[0076] Comparative Example 5:
[0077] The difference from Example 3 is that the method of Example 3 is used to prepare the four-element rare earth oxide stabilized zirconium oxide material ZrO2-4.9La2O3-4.5Sm2O3-5.3Er2O3-5.2Dy2O3 ceramic material and spray powder;
[0078] Comparative Example 6:
[0079] The difference from Example 4 is that the method of Example 4 is used to prepare a four-element rare earth oxide stabilized zirconium oxide coating: ZrO2-4.9La2O3-4.5Sm2O3-5.3Er2O3-5.2Dy2O3 ceramic coating;
[0080] like Figure 2 and 3 As shown in Table 1, the thermal conductivity, thermal expansion coefficient, and water-cooled thermal cycle life of the rare earth stabilized zirconia ceramic materials prepared in the above embodiments and comparative examples were tested at 1100°C. The results are shown in Table 1. 3+ , B 4+ The thermal conductivity of the multi-component rare earth stabilized zirconia ceramic material is ≤1.0W / (m*K), which is much lower than that of Comparative Example 1, Comparative Example 3 and Comparative Example 5, and the thermal expansion coefficient is greater than 11.0×10 -6 K -1, which is greater than that of Comparative Example 1, Comparative Example 3 and Comparative Example 5. At the same time, the water cooling thermal cycle life of its thermal barrier coating is also higher than that of Comparative Example 2, Comparative Example 4 and Comparative Example 6. The comprehensive data show that A 3+ , B 4+ Multi-element composite stabilized zirconia greatly reduces the thermal conductivity of zirconia, increases the thermal expansion coefficient of the material, and makes it closer to the thermal expansion coefficient of the matrix material Ni high-temperature alloy, which helps to improve the thermal cycle life of the material.
[0081] Table 1 shows the thermal conductivity, thermal expansion coefficient and water cooling thermal cycle number of Examples 1 to 4 and Comparative Examples 1 to 6 at 1100°C.
[0082]
[0083]
[0084] The present invention distorts the ZrO2 lattice by doping with trivalent rare earth elements, forming more point defects, increasing the bond length of the XO bond and reducing the population, causing the lattice vibration frequency to decrease and the phonon scattering to intensify, thereby reducing the thermal diffusion coefficient of the material, reducing the thermal conductivity, and improving the thermal insulation performance of the coating material. However, the increase in the bond length of the XO bond will cause a decrease in the thermal expansion coefficient and weaken the thermal shock resistance of the coating. To this end, by replacing the tetravalent metal ions equivalent to the zirconium ions, the strength of the XO bond is reduced, thereby increasing the thermal expansion coefficient, enhancing the thermal shock resistance of the coating, and improving the service life of the material. The A 3+ , B 4+ The thermal conductivity of multi-component composite stabilized zirconia thermal barrier ceramic material at 1100℃ is ≤1.0W / (m*K), and the thermal expansion coefficient is >11.0×10 -6 K -1 .
[0085] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A multi-component composite stabilized zirconia thermal barrier coating material, characterized in that: The thermal barrier coating material comprises a tetravalent B element and a trivalent rare earth oxide. The chemical formula of the thermal barrier coating material is (Zr 1-x B x )O2-y%wtA2O3, wherein x is the content of doped tetravalent B element, y is the mass percentage of doped trivalent rare earth oxide, wherein 0.1≤x≤0.3, 10≤y≤25, the particle size of the thermal barrier coating material is 25-75μm, the trivalent rare earth oxide A2O3 is any four or five of Gd2O3, Yb2O3, Nd2O3, Pr2O3, Sm2O3, Er2O3, and Dy2O3; the oxide BO2 of the tetravalent B element is any two or three of TiO2, HfO2, CeO2, and MoO2.
2. A multi-component composite stabilized zirconia thermal barrier coating, characterized in that: It includes a metal bonding layer and a thermal barrier ceramic layer, wherein the thermal barrier ceramic layer includes a tetravalent B element and a trivalent rare earth oxide, and the chemical formula of the thermal barrier ceramic layer is (Zr 1-x B x )O2-y%wtA2O 33 , wherein x is the content of doped tetravalent B element, y is the mass percentage of doped trivalent rare earth oxide, wherein 0.1≤x≤0.3, 10≤y≤25, the metal bonding layer comprises one or more of CoNiCrAlY, NiCoCrAlY or NiCoCrAlTaY, the thickness of the metal bonding layer is 100-200 μm, and the metal bonding layer is prepared on the alloy substrate by supersonic flame spraying; and the surface thermal barrier ceramic layer is prepared on the surface of the metal bonding layer by atmospheric plasma spraying.
3. A method for preparing a multi-component composite stabilized zirconium oxide thermal barrier coating material, characterized in that , the method for preparing the coating material as claimed in claim 1 comprises: 1) weighing rare earth oxide A2O3, tetravalent metal oxide BO2 and ZrOCl2·8H2O in a stoichiometric ratio of (0.1-0.3):(10-25), dissolving the oxide in diluted concentrated nitric acid or concentrated sulfuric acid, and dissolving ZrOCl2·8H2O in deionized water; 2) mixing the two solutions, adding polyethylene glycol dispersant, and stirring with a glass rod to obtain a clear mixed solution; 3) Under ultrasonic vibration environment, reversely titrate the mixed solution into an ammonia solution to form a colloidal precipitate, maintain the pH value of the ammonia solution ≥ 10 during the titration process, and let it stand for 24 hours after the titration is completed; 4) centrifuging and washing the colloidal precipitate with deionized water at a centrifugal speed of 5000-8000 r / min until the pH value of the supernatant after centrifugation is neutral, washing it with anhydrous ethanol, and drying it in an oven to obtain a precursor powder; 5) sintering the precursor powder in an air environment at 1200° C. to 1400° C. for 5 to 8 hours to obtain a composite rare earth stabilized zirconia thermal barrier ceramic material; 6) wet-milling the composite rare earth stabilized zirconia thermal barrier ceramic material to obtain a slurry, wherein the ball milling medium is anhydrous ethanol and the ball milling beads are made of zirconia; 7) placing the slurry in a drying oven for drying to obtain powder, the drying temperature is 80-100° C., and the drying time is 15-20 hours; 8) adding the dried powder to a ball mill for mixing to obtain a mixed slurry; 9) subjecting the mixed slurry to centrifugal spray granulation to obtain agglomerated powder; 10) Sintering, crushing and screening the agglomerated powder to obtain the multi-component composite stabilized zirconia thermal barrier coating material; In step (6), the ball milling speed is 400-600 r / min, and the ball milling time is 20-30 h; In step (8), the ball milling speed is 300-500 r / min, and the ball milling mixing time is 15-25 h; In step (8), 15-30 wt.% of deionized water, 3-6 wt.% of polyacrylic acid and 2-5 wt.% of polyvinyl alcohol are added; In step (9), the centrifugal speed during the centrifugal spray granulation is 15,000 to 20,000 rpm, the air inlet temperature is 250 to 320° C., the air outlet temperature is 100 to 150° C., and the feed rate is 30 to 45 rpm. In step (10), the sintering temperature is 1200-1400° C., and the sintering holding time is 2-6 hours.