A high-strength environmentally friendly aerated brick and preparation method thereof

By using rice husk ash, rice husk lignin and rice husk filter slag as reinforced fillers in aerated bricks, and alkali modification and sulfonation modification, the problem of improving compressive strength and environmental protection of aerated bricks is solved, and the problem of improving the compressive strength and environmental protection of aerated bricks is achieved. It has the dual goals of high strength and environmental protection, and is suitable for the material needs of high-rise buildings.

CN117658665BActive Publication Date: 2024-11-05ZHAOQING XINJINHUI BUILDING MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311410776.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-28
Publication Date
2024-11-05
Estimated Expiration
2043-10-28

AI Technical Summary

Technical Problem

There is room for improvement in compressive strength and environmental protection of existing aerated bricks, and there are environmental pollution problems during the production process, making it difficult to meet the dual needs of building materials for high strength and environmental protection.

Method used

Use rice husk ash, rice husk lignin and rice husk filter slag as reinforced fillers. Through specific extraction and modification treatment, combined with cement, gypsum powder, fly ash and other raw materials, high-strength environmentally friendly gas bricks are prepared to improve compressive strength. and frost resistance, and improve impermeability through alkali modification and sulfonation modification.

Benefits of technology

It significantly improves the compressive strength and frost resistance of aerated bricks, reduces environmental pollution during the production process, achieves higher environmental protection and performance optimization, and is suitable for the use needs of high-rise buildings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a high-strength environmentally friendly aerated brick and a preparation method thereof, and relates to the technical field of building material preparation. A high-strength environmentally friendly aerated brick comprises 15-30 parts of cement, 12-20 parts of quicklime, 20-25 parts of gypsum powder, 80-90 parts of fly ash, 15-30 parts of sand and gravel, 40-60 parts of water, 4-8 parts of aluminum powder paste, 3-6 parts of coupling agent, 0.2-0.5 parts of water reducer, 0.7-1.5 parts of foam stabilizer, and 25-65 parts of rice husk extract. The rice husk extract includes rice husk ash, rice husk lignin and rice husk filter residue. The weight ratio of rice husk ash, rice husk lignin and rice husk filter residue is (10-15):1:(4-10). The present invention improves the compressive strength of aerated bricks by adding a certain amount of rice husk extract. Rice husk is a by-product of rice processing. Filling with rice husk extract can fully play the role of waste utilization, making the production of aerated bricks more green and environmentally friendly, and improving the environmental protection of aerated bricks.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of building material preparation, and in particular to a high-strength environmentally friendly aerated brick and a preparation method thereof. Background Art

[0002] Aerated bricks, also known as aerated concrete blocks, are widely used. They are mainly used in mechanical workshops and civil buildings as wall materials, infill walls, floor slabs, roof panels and other load-bearing wall materials, as well as non-load-bearing materials and surrounding infill walls.

[0003] Because aerated bricks have the characteristics of light weight, good thermal insulation, strong earthquake resistance, good processing performance, and certain high temperature resistance, good sound insulation performance, and strong adaptability, aerated bricks have become the leading product in the building materials industry. As the country gradually bans the use of solid clay bricks, they are gradually replaced by aerated concrete blocks and autoclaved bricks.

[0004] With the development of the construction industry, buildings are getting taller and taller, so people have higher requirements for the strength and other performance of building materials such as aerated bricks. In addition, with the continuous improvement of people's living standards, the requirements for the environment are getting higher and higher, and there are higher requirements for the environmental protection of building materials, and the pollution to the environment is reduced as much as possible during the production of building materials. Therefore, it is particularly important to further improve the filler of aerated bricks, so that aerated bricks have higher strength, more environmentally friendly production process, and more in line with the current needs of society. Summary of the invention

[0005] In order to further improve the strength of aerated bricks, the present application provides a high-strength environmentally friendly aerated brick and a preparation method thereof.

[0006] In the first aspect, the present application provides a high-strength environmentally friendly aerated brick, which adopts the following technical solution:

[0007] A high-strength environmentally friendly aerated brick, comprising the following raw materials in parts by weight:

[0008] 15-30 parts of cement;

[0009] 12-20 parts of quicklime;

[0010] 20-25 parts of gypsum powder;

[0011] 80-90 parts of fly ash;

[0012] 15-30 parts of sand and gravel;

[0013] 40-60 parts of water;

[0014] 4-8 parts of aluminum paste;

[0015] 3-6 parts of coupling agent;

[0016] Water reducing agent 0.2-0.5 parts;

[0017] Foam stabilizer 0.7-1.5 parts;

[0018] 25-65 parts of rice husk extract;

[0019] The rice husk extract comprises rice husk ash, rice husk lignin and rice husk filter residue, wherein the weight ratio of the rice husk ash, the rice husk lignin and the rice husk filter residue is (10-15):1:(4-10).

[0020] By adopting the above technical scheme, aerated bricks with a certain amount of rice husk extracts such as rice husk ash, rice husk lignin, and rice husk filter residue are added, which is not only conducive to improving the compressive strength of aerated bricks, but also after multiple freeze-thaw cycles, the aerated bricks can remain intact and still maintain good compressive strength, which is conducive to improving the frost resistance and durability of aerated bricks. Since most of the other compounds in the rice husk that are not cellulose and ash can be removed after rice husk ash, rice husk lignin, and rice husk filter residue are extracted from the rice husk, it is conducive to preventing other compound components contained in the rice husk from affecting the gel reaction of the aerated brick slurry. Therefore, by extracting effective extracts such as rice husk ash, rice husk lignin, and rice husk filter residue from the rice husk, it is conducive to making rice husk extracts such as rice husk ash, rice husk lignin, and rice husk filter residue fully play their reinforcing role when used as reinforcing fillers, which can effectively improve the compressive strength of aerated bricks.

[0021] Furthermore, rice husk is a by-product of rice processing, and rice husk ash, rice husk lignin and rice husk residue are extracted from rice husk, which fully plays the role of waste utilization. At the same time, using rice husk extract to replace traditional limestone as a reinforcing filler is beneficial to reduce the pollution caused by the use and production of limestone, making the production of aerated bricks more green and environmentally friendly, and improving the environmental protection of aerated bricks.

[0022] Optionally, the method for extracting rice husk ash is:

[0023] A1. Wash the rice husks with tap water and soak them in water for 10-12 hours, then boil them with 10% HCl solution for 4 hours. After boiling, take out the rice husks and dry them.

[0024] A2. The dried rice husk is placed in a muffle furnace, heated to 500-550° C., and calcined for 3-4 hours to obtain the obtained product; wherein the extraction method of the rice husk lignin and the rice husk residue is as follows:

[0025] B1. First, grind the rice husk to obtain rice husk powder, then fully mix the rice husk powder, ethanol and an appropriate amount of water, heat to 80-90° C., and stir to react for 3.5-5 hours;

[0026] B2. After the reaction is completed, the rice husk filtrate and the rice husk residue are separated by filtration, and the rice husk filtrate is evaporated to dryness to obtain rice husk lignin.

[0027] By adopting the above technical scheme, rice husk ash, rice husk lignin and rice husk residue can be extracted from rice husk accordingly without too many complicated raw materials and equipment. The extraction steps are simple and convenient, which is conducive to subsequent mass production.

[0028] Optionally, the weight ratio of the rice husk ash, the rice husk lignin and the rice husk residue is (13-14):1:(4-6).

[0029] By adopting the above technical solution, when the weight ratio of rice husk ash, rice husk lignin and rice husk filter residue is in the range of (13-14):1:(4-6), the compressive strength and frost resistance of the aerated brick are better, and after multiple freeze-thaw cycles, the compressive strength loss rate and mass loss rate of the aerated brick are low. Appropriately reducing the amount of rice husk filter residue added is conducive to preventing other compounds remaining in the rice husk filter residue from causing gel reaction of the aerated brick slurry, thereby causing the performance of the aerated brick to deteriorate.

[0030] Optionally, part of the rice husk ash is alkali-modified rice husk ash, and the weight ratio between the rice husk ash and the alkali-modified rice husk ash is 1:(1.2-1.5).

[0031] By adopting the above technical scheme, alkali-modified rice husk ash can significantly improve the anti-permeability of aerated bricks, and the compressive strength of aerated bricks is not greatly improved. When rice husk ash and alkali-modified rice husk ash are mixed with each other and the mixing weight ratio is 1: (1.2-1.5), the comprehensive performance of aerated bricks is relatively excellent, with both high compressive strength and good anti-permeability.

[0032] Optionally, the preparation method of the alkali-modified rice husk ash is:

[0033] C1. Mix the rice husk ash with a sodium hydroxide solution having a concentration of 10%-12% in a ratio of 1:(0.8-1), then keep the reaction at a constant temperature of 80° C.-100° C. for 5-6 hours, filter the residue to obtain an alkali-modified rice husk ash liquid, and evaporate to dryness to obtain an alkali-modified rice husk ash.

[0034] By adopting the above technical solution, rice husk ash can be alkali-modified without too many complicated raw materials and equipment. The alkali modification step is simple and convenient, which is conducive to subsequent mass production.

[0035] Optionally, the rice husk lignin is sulfonated modified rice husk lignin.

[0036] By adopting the above technical solution, the rice husk lignin is sulfonated and modified, which is beneficial to improve the dispersibility of rice husk lignin in aerated bricks, so that the rice husk lignin can be fully and evenly dispersed in the aerated bricks, which is beneficial to improve the mechanical properties of the aerated bricks. In addition, the sulfonated modified rice husk lignin may have a certain water-reducing effect, which can not only reduce the addition of water-reducing agent in a suitable mixing system, which is beneficial to reduce production costs, but also further improve the mechanical properties of aerated bricks.

[0037] Optionally, the preparation method of the sulfonated modified rice husk lignin comprises:

[0038] D1. Adding sodium sulfite to the rice husk lignin, heating to 160-180° C., reacting for 1.5-2 hours in an alkaline environment, and obtaining sulfonated modified rice husk lignin.

[0039] By adopting the above technical solution, rice husk lignin can be sulfonated without too many complicated raw materials and equipment. The sulfonation modification steps are simple and convenient, which is conducive to subsequent large-scale production.

[0040] Optionally, the rice husk residue is pretreated with a toluene-2,4-diisocyanate solution before mixing, wherein the toluene-2,4-diisocyanate solution comprises toluene-2,4-diisocyanate and a solvent.

[0041] By adopting the above technical scheme, after pretreating the rice husk residue with toluene-2,4-diisocyanate solution, the hydrophilicity of the rice husk cellulose in the rice husk residue can be reduced, so as to reduce the agglomeration of the rice husk cellulose itself, so that the pretreated rice husk residue can be fully and evenly dispersed in the aerated brick slurry, which is beneficial to further improve the compressive strength, frost resistance and impermeability of the aerated brick.

[0042] Optionally, the coupling agent is a mixture of KH550 silane coupling agent and KH560 silane coupling agent, and the weight ratio of the KH550 silane coupling agent to the KH560 silane coupling agent is 1:(2.5-4); the water reducer is a polycarboxylic acid-based water reducer, and the foam stabilizer is a silicone resin polyether foam stabilizer.

[0043] By adopting the above technical scheme, KH550 silane coupling agent is mainly used for the surface treatment of inorganic fillers, and KH560 silane coupling agent is mainly used for the surface treatment of reinforcing agents and inorganic fillers. The two are mixed according to the weight ratio of 1: (2.5-4), which is beneficial to improve the compatibility between fillers such as gypsum powder, fly ash, and rice husk extract and aerated brick slurry, so that the fillers are fully dispersed and mixed in the aerated brick slurry, which is beneficial to improve the compressive strength of aerated bricks. Polycarboxylic acid-based water reducers can reduce the water used in aerated brick slurry, and have outstanding advantages such as low dosage, good collapse retention performance, and low concrete shrinkage. Silicone resin polyether foam stabilizer can control the structural stability of the bubble liquid film, so that the bubbles can be distributed in an orderly manner, improve the pore structure in aerated bricks, reduce string holes, and have obvious foam stabilization effects, which is practical and convenient.

[0044] In the second aspect, the present application also provides a method for preparing a high-strength environmentally friendly aerated brick, which adopts the following technical solution:

[0045] A method for preparing a high-strength environmentally friendly aerated brick comprises the following steps:

[0046] E1. First, mix cement, quicklime, gypsum powder and fly ash, and grind them into 50-100 mesh cement powder in a ball mill. Then transfer the cement powder to a cement mixing tank, add sand, coupling agent, water reducer, foam stabilizer and rice husk extract, and mix them with the cement powder. Add water and aluminum powder paste, stir evenly to obtain slurry, and then pour the slurry into a mold, wait for the slurry to cool and solidify to obtain the embryo brick;

[0047] E2. Put the green brick obtained in E1 into a steam curing kettle and evacuate it. Then, evenly introduce steam within 1.8-2 hours to make the temperature in the steam curing kettle reach 170-180 degrees Celsius and the pressure in the kettle reach 1.0-1.2MPa. Keep the constant temperature and pressure for 9-12 hours.

[0048] E3. After the reaction is completed, release the steam slowly and evenly. When the temperature in the steam curing kettle drops to 50°C, take out the brick from the steam curing kettle and place it at room temperature and pressure for 28-30 days to obtain aerated bricks.

[0049] By adopting the above technical solution, the rice husk extract can be fully mixed in the slurry of the aerated brick, so that aerated bricks with high strength and environmental protection can be produced. Moreover, the preparation steps are simple and convenient, which is conducive to subsequent mass production.

[0050] In summary, the implementation scheme of the present application has at least one of the following beneficial effects:

[0051] 1. By adding rice husk extracts such as rice husk ash, rice husk lignin and rice husk filter residue in a certain proportion, it is not only beneficial to improve the compressive strength of aerated bricks, but also to enable aerated bricks to maintain good compressive strength after multiple freeze-thaw cycles, which is beneficial to improve the durability of aerated bricks.

[0052] 2. By extracting rice husk ash, rice husk lignin and rice husk residue from rice husk and then adding them into aerated bricks as reinforcing fillers, it is helpful to prevent other compound components contained in rice husk from affecting the gel reaction of aerated brick slurry, so that rice husk extracts such as rice husk ash, rice husk lignin and rice husk residue can fully play their reinforcing role when used as reinforcing fillers, and can effectively improve the compressive strength of aerated bricks.

[0053] 3. By alkali-modifying rice husk ash and mixing rice husk ash with alkali-modified rice husk ash in a certain proportion, it is beneficial to make the aerated brick have both high compressive strength and good anti-permeability performance.

[0054] 4. Sulfonation modification of rice husk lignin is beneficial to improve the dispersibility of rice husk lignin in aerated bricks and improve the mechanical properties of aerated bricks.

[0055] 5. By pre-treating the rice husk residue, the pre-treated rice husk residue can be fully and evenly dispersed in the aerated brick slurry, which is beneficial to further improve the compressive strength, frost resistance and impermeability of the aerated brick. DETAILED DESCRIPTION

[0056] The present application is further described in detail below with reference to embodiments and comparative examples.

[0057] The cement was purchased from Shandong Zhenxing Cement Co., Ltd. with the specification of P.O42.5 grade.

[0058] The gypsum powder was purchased from Jinan Zhongqi Chemical Co., Ltd., with an average mesh size of 300 meshes.

[0059] Aluminum powder paste was purchased from Shandong Sanpin Aluminum Technology Co., Ltd., model GLS-65.

[0060] The water reducing agent is a polycarboxylic acid water reducing agent.

[0061] The foam stabilizer is a silicone resin polyether foam stabilizer.

[0062] Rice husk extract can be extracted from rice husk.

[0063] Preparation Example

[0064] Preparation Example 1

[0065] The extraction method of rice husk ash is:

[0066] A1. Wash the rice husks with tap water and soak them in water for 12 hours, then boil them with 10% HCl solution for 3 hours. After boiling, take out the rice husks and dry them.

[0067] A2. The dried rice husk is placed in a muffle furnace and heated to 550° C., and calcined for 3 hours to obtain the obtained product.

[0068] The extraction method of rice husk lignin and rice husk residue is as follows:

[0069] B1. First, grind the rice husk to obtain rice husk powder, then fully mix the rice husk powder, ethanol and an appropriate amount of water, heat to 80°C, and stir to react for 5 hours;

[0070] B2. After the reaction is completed, the rice husk filtrate and the rice husk residue are separated by filtration, and then the rice husk filtrate is evaporated to dryness to obtain rice husk lignin and rice husk residue.

[0071] Preparation Example 2

[0072] The extraction method of rice husk ash is:

[0073] A1. Wash the rice husks with tap water and soak them in water for 10 hours, then boil them with 10% HCl solution for 4 hours. After boiling, take out the rice husks and dry them.

[0074] A2. The dried rice husk is placed in a muffle furnace and heated to 500° C., and calcined for 4 hours to obtain the obtained product.

[0075] The extraction method of rice husk lignin and rice husk residue is as follows:

[0076] B1. First, grind the rice husk to obtain rice husk powder, then fully mix the rice husk powder, ethanol and an appropriate amount of water, heat to 90°C, and stir to react for 3.5h;

[0077] B2. After the reaction is completed, the rice husk filtrate and the rice husk residue are separated by filtration, and then the rice husk filtrate is evaporated to dryness to obtain rice husk lignin and rice husk residue.

[0078] Example

[0079] Example 1

[0080] A high-strength environmentally friendly aerated brick, comprising the following raw materials:

[0081] 30kg cement, 12kg quicklime, 25kg gypsum powder, 90kg fly ash, 30kg sand and gravel, 60kg water, 8kg aluminum paste, 5kg coupling agent, 0.5kg polycarboxylic acid water reducer, 1.5kg silicone resin polyether foam stabilizer, and 38kg rice husk extract.

[0082] The coupling agent is a mixture of KH550 silane coupling agent and KH560 silane coupling agent. Specifically, the weight ratio of KH550 silane coupling agent to KH560 silane coupling agent is 1:2.5.

[0083] Among them, the rice husk extract is a mixture of rice husk ash, rice husk lignin and rice husk residue produced when extracting rice husk lignin. Specifically, rice husk ash, rice husk lignin and rice husk residue are prepared by Preparation Example 1, and the weight ratio of rice husk ash, rice husk lignin and rice husk residue is 15:1:3, that is, the rice husk extract contains 30kg of rice husk ash, 2kg of rice husk lignin and 8kg of rice husk residue.

[0084] A method for preparing a high-strength environmentally friendly aerated brick comprises the following steps:

[0085] E1. First, cement, quicklime, gypsum powder and fly ash are fully mixed according to the proportion, and then sent into a ball mill to grind into 50-100 mesh cement powder. Then, the cement powder is transferred to a cement mixing tank, and then sand, coupling agent, water reducer, foam stabilizer and rice husk extract are added and fully mixed with the cement powder. Water and aluminum powder paste are added and stirred to obtain slurry. Then, the slurry is poured into a mold, and the embryo brick is obtained after the slurry is cooled and solidified;

[0086] E2. Put the green brick obtained in E1 into a steam curing kettle and evacuate it. Then, evenly introduce steam within 1.8 hours to make the temperature in the steam curing kettle reach 170 degrees Celsius and the pressure in the kettle reach 1.0 MPa. Keep the constant temperature and pressure for 9 hours.

[0087] E3. After the reaction is completed, release the steam slowly and evenly. When the temperature in the steam-curing kettle drops to 50°C, take out the brick from the steam-curing kettle and place it at room temperature and pressure for 28 days to obtain aerated bricks.

[0088] Example 2

[0089] A high-strength environmentally friendly aerated brick, comprising the following raw materials:

[0090] 15kg cement, 20kg quicklime, 20kg gypsum powder, 80kg fly ash, 15kg sand and gravel, 40kg water, 4kg aluminum paste, 3kg coupling agent, 0.2kg polycarboxylic acid water reducer, 0.7kg silicone resin polyether foam stabilizer, and 63kg rice husk extract.

[0091] The coupling agent is a mixture of KH550 silane coupling agent and KH560 silane coupling agent. Specifically, the weight ratio of KH550 silane coupling agent to KH560 silane coupling agent is 1:4.

[0092] Among them, the rice husk extract is a mixture of rice husk ash, rice husk lignin and rice husk residue produced when extracting rice husk lignin. Specifically, rice husk ash, rice husk lignin and rice husk residue are prepared by Preparation Example 2, and the weight ratio of rice husk ash, rice husk lignin and rice husk residue is 10:1:10, that is, the rice husk extract contains 30kg of rice husk ash, 3kg of rice husk lignin and 30kg of rice husk residue.

[0093] A method for preparing a high-strength environmentally friendly aerated brick comprises the following steps:

[0094] E1. First, cement, quicklime, gypsum powder and fly ash are fully mixed according to the proportion, and then sent into a ball mill to grind into 50-100 mesh cement powder. Then, the cement powder is transferred to a cement mixing tank, and then sand, coupling agent, water reducer, foam stabilizer and rice husk extract are added and fully mixed with the cement powder. Water and aluminum powder paste are added and stirred to obtain slurry. Then, the slurry is poured into a mold, and the embryo brick is obtained after the slurry is cooled and solidified;

[0095] E2. Put the green brick obtained in E1 into a steam curing kettle and evacuate it. Then, introduce steam evenly within 2 hours to make the temperature in the steam curing kettle reach 175 degrees Celsius and the pressure in the kettle reach 1.1 MPa. Keep the constant temperature and pressure for 10 hours.

[0096] E3. After the reaction is completed, release the steam slowly and evenly. When the temperature in the steam-curing kettle drops to 50°C, take out the brick from the steam-curing kettle and place it at room temperature and pressure for 29 days to obtain aerated bricks.

[0097] Example 3

[0098] A high-strength environmentally friendly aerated brick, comprising the following raw materials:

[0099] 20kg cement, 18kg quicklime, 20kg gypsum powder, 30kg fly ash, 15kg sand and gravel, 50kg water, 6kg aluminum paste, 4kg coupling agent, 0.4kg polycarboxylic acid water reducer, 0.8kg silicone resin polyether foam stabilizer, and 47.5kg rice husk extract.

[0100] The coupling agent is a mixture of KH550 silane coupling agent and KH560 silane coupling agent. Specifically, the weight ratio of KH550 silane coupling agent to KH560 silane coupling agent is 1:3.

[0101] Among them, the rice husk extract is a mixture of rice husk ash, rice husk lignin and rice husk residue produced when extracting rice husk lignin. Specifically, rice husk ash, rice husk lignin and rice husk residue are prepared by Preparation Example 1, and the weight ratio of rice husk ash, rice husk lignin and rice husk residue is 11:1:7, that is, the rice husk extract contains 27.5 kg of rice husk ash, 2.5 kg of rice husk lignin and 17.5 kg of rice husk residue.

[0102] A method for preparing a high-strength environmentally friendly aerated brick comprises the following steps:

[0103] E1. First, cement, quicklime, gypsum powder and fly ash are fully mixed according to the proportion, and then sent into a ball mill to grind into 50-100 mesh cement powder. Then, the cement powder is transferred to a cement mixing tank, and then sand, coupling agent, water reducer, foam stabilizer and rice husk extract are added and fully mixed with the cement powder. Water and aluminum powder paste are added and stirred to obtain slurry. Then, the slurry is poured into a mold, and the embryo brick is obtained after the slurry is cooled and solidified;

[0104] E2. Put the green brick obtained in E1 into a steam curing kettle and evacuate it. Then, evenly introduce steam within 2 hours to make the temperature in the steam curing kettle reach 180 degrees Celsius and the pressure in the kettle reach 1.2 MPa. Keep the constant temperature and pressure for 12 hours.

[0105] E3. After the reaction is completed, release the steam slowly and evenly. When the temperature in the steam curing kettle drops to 50°C, take out the brick from the steam curing kettle and place it at room temperature and pressure for 30 days to obtain aerated bricks.

[0106] Example 4

[0107] A high-strength environmentally friendly aerated brick, which is different from Example 3 in that the weight ratios of rice husk ash, rice husk lignin and rice husk filter residue are different.

[0108] In this embodiment, the weight ratio of rice husk ash, rice husk lignin and rice husk residue is 14:1:4, that is, the rice husk extract contains 35 kg of rice husk ash, 2.5 kg of rice husk lignin and 10 kg of rice husk residue.

[0109] Example 5

[0110] A high-strength environmentally friendly aerated brick, which differs from Example 4 in that all rice husk ash is replaced with alkali-modified rice husk ash in equal amounts, that is, the rice husk extract contains 35 kg of modified rice husk ash, 2.5 kg of rice husk lignin, and 10 kg of rice husk filter residue.

[0111] Specifically, the preparation method of alkali-modified rice husk ash is:

[0112] C1. Mix rice husk ash with 12% sodium hydroxide solution in a ratio of 1:0.8, then keep the reaction at 80° C. for 5 hours, filter the residue to obtain alkali-modified rice husk ash liquid, and evaporate to dryness to obtain alkali-modified rice husk ash.

[0113] Example 6

[0114] A high-strength environmentally friendly aerated brick, which differs from Example 4 in that part of the rice husk ash is replaced with alkali-modified rice husk ash in equal amounts.

[0115] Specifically, the preparation method of alkali-modified rice husk ash is:

[0116] C1. Mix rice husk ash with 12% sodium hydroxide solution in a ratio of 1:0.8, then keep the reaction at 80° C. for 5 hours, filter the residue to obtain alkali-modified rice husk ash liquid, and evaporate to dryness to obtain alkali-modified rice husk ash.

[0117] In this embodiment, the weight ratio of rice husk ash to alkali-modified rice husk ash is 1:1.2, that is, the rice husk extract contains 16 kg of rice husk ash, 19 kg of modified rice husk ash, 2.5 kg of rice husk lignin, and 10 kg of rice husk residue.

[0118] Example 7

[0119] A high-strength environmentally friendly aerated brick, which differs from Example 6 in that: rice husk lignin is replaced with sulfonated modified rice husk lignin in equal amounts, that is, the rice husk extract contains 16 kg of rice husk ash, 19 kg of modified rice husk ash, 2.5 kg of sulfonated modified rice husk lignin, and 10 kg of rice husk filter residue.

[0120] Specifically, the preparation method of sulfonated modified rice husk lignin is:

[0121] D1. Adding sodium sulfite to the rice husk lignin, heating to 180° C., reacting for 2 hours in an alkaline environment, and obtaining sulfonated modified rice husk lignin.

[0122] Example 8

[0123] A high-strength environmentally friendly aerated brick, which is different from Example 7 in that the amount of polycarboxylic acid type water reducing agent added is different.

[0124] In this embodiment, 0.2 kg of polycarboxylic acid type water reducer is added.

[0125] Example 9

[0126] A high-strength environmentally friendly aerated brick, which is different from Example 8 in that the rice husk filter residue is treated with a toluene-2,4 diisocyanate solution before being mixed with cement powder. The toluene-2,4 diisocyanate solution is composed of toluene-2,4 diisocyanate and ethyl acetate solvent, and the mass concentration of toluene-2,4 diisocyanate is 1%.

[0127] Specifically, the pretreatment steps are: adding rice husk filter residue to toluene-2,4-diisocyanate solution, stirring and dispersing at 40° C. for 2 hours, filtering and placing the filter residue in an oven, and drying at 60° C. to obtain pretreated rice husk filter residue.

[0128] In this embodiment, the rice husk extract comprises 16 kg of rice husk ash, 19 kg of modified rice husk ash, 2.5 kg of sulfonated modified rice husk lignin, and 10 kg of pretreated rice husk residue.

[0129] Example 10

[0130] A high-strength environmentally friendly aerated brick, which differs from Example 9 in that all alkali-modified rice husk ash is replaced with rice husk ash in equal amounts, that is, the rice husk extract contains 35 kg of rice husk ash, 2.5 kg of sulfonated modified rice husk lignin, and 10 kg of pretreated rice husk residue.

[0131] Embodiment 11

[0132] A high-strength environmentally friendly aerated brick, which is different from Example 4 in that the rice husk filter residue is first treated with a toluene-2,4 diisocyanate solution before being mixed with cement powder. The toluene-2,4 diisocyanate solution is composed of toluene-2,4 diisocyanate and ethyl acetate solvent, and the mass concentration of toluene-2,4 diisocyanate is 1%.

[0133] Specifically, the pretreatment steps are: adding rice husk filter residue to toluene-2,4-diisocyanate solution, stirring and dispersing at 40° C. for 2 hours, filtering and placing the filter residue in an oven, and drying at 60° C. to obtain pretreated rice husk filter residue.

[0134] In this embodiment, the rice husk extract comprises 35 kg of rice husk ash, 2.5 kg of rice husk lignin, and 10 kg of pretreated rice husk residue.

[0135] Example 12

[0136] A high-strength environmentally friendly aerated brick, which differs from Example 11 in that a portion of rice husk ash is replaced with alkali-modified rice husk ash in equal amounts.

[0137] Specifically, the preparation method of alkali-modified rice husk ash is:

[0138] C1. Mix rice husk ash with 10% sodium hydroxide solution in a ratio of 1:1, then keep the reaction at 100° C. for 6 hours, filter the residue to obtain alkali-modified rice husk ash liquid, and evaporate to dryness to obtain alkali-modified rice husk ash.

[0139] In this embodiment, the weight ratio of rice husk ash to alkali-modified rice husk ash is 1:1.5, that is, the rice husk extract contains 14 kg of rice husk ash, 21 kg of modified rice husk ash, 2.5 kg of rice husk lignin, and 10 kg of pretreated rice husk residue.

[0140] Embodiment 13

[0141] A high-strength environmentally friendly aerated brick, which differs from Example 12 in that an equal amount of rice husk lignin is replaced with sulfonated modified rice husk lignin, that is, the rice husk extract contains 14 kg of rice husk ash, 21 kg of modified rice husk ash, 2.5 kg of sulfonated modified rice husk lignin, and 10 kg of pretreated rice husk residue.

[0142] Specifically, the preparation method of sulfonated modified rice husk lignin is:

[0143] D1. Adding sodium sulfite to the rice husk lignin, heating to 150° C., reacting for 1.5 hours in an alkaline environment, and obtaining sulfonated modified rice husk lignin.

[0144] Comparative Example

[0145] Comparative Example 1

[0146] An aerated brick, which is different from Example 4 in that no rice husk extract is added, and the rice husk extract is completely replaced by an equal amount of limestone.

[0147] Comparative Example 2

[0148] An aerated brick, which differs from Example 4 in that the rice husk extract is completely replaced with an equal amount of rice husk.

[0149] Comparative Example 3

[0150] An aerated brick, which differs from Example 4 in that the rice husk lignin and rice husk residue in the rice husk extract are all replaced with an equal amount of rice husk, and the amount of rice husk ash added remains unchanged.

[0151] Performance test data

[0152] Preparation of samples to be tested: The aerated bricks prepared in Examples 1-12 and Comparative Examples 1-3 were cast into standard test blocks of 600 mm*250 mm*250 mm respectively.

[0153] (1) Compressive strength test: Sampling test is carried out according to Chapter 4 Mechanical Properties of GB / T 11969-2020 Test Methods for Properties of Autoclaved Aerated Concrete, and the compressive strength (MPa) is recorded.

[0154] (2) Frost resistance test: According to Chapter 6 of GB / T 11969-2020 Test Method for Performance of Autoclaved Aerated Concrete, sampling test shall be carried out. After the freeze-thaw cycle is completed, the compressive strength loss rate (%) and mass loss rate (%) shall be recorded. If damage occurs during the freeze-thaw process, the damage shall be recorded.

[0155] (3) Water seepage test: Sampling test was conducted according to the water seepage test method in Appendix D of GB / T 29062-2012 Autoclaved Foam Concrete Bricks and Blocks. The test time was 8 hours and the maximum water seepage depth was recorded.

[0156] Table 1 Performance test data of aerated bricks

[0157]

[0158]

[0159] Combining Example 4 with Comparative Example 1 and the data in Table 1, it can be seen that compared with traditional aerated bricks filled with limestone, aerated bricks with rice husk extracts such as rice husk ash, rice husk lignin and rice husk residue added, under the combined action of rice husk extracts, not only have better compressive strength and impermeability, but also after multiple freeze-thaw cycles, the aerated bricks can remain intact and have better antifreeze performance.

[0160] Combining Example 4 with Comparative Examples 1-3 and the data in Table 1, it can be seen that: although the compressive strength, frost resistance and impermeability of aerated bricks are improved to a certain extent by directly filling and modifying aerated bricks with rice husks, the improvement is not large. This may be because the components contained in rice husks are complex. In addition to crude fiber, hemicellulose and ash, they also contain organic compounds such as crude protein and crude fat, as well as nitrogen-free extracts such as starch and monosaccharides. These other compounds that are not cellulose and ash may affect the gel reaction of the aerated brick slurry, thereby resulting in a decrease in the compressive strength, frost resistance and impermeability of the aerated bricks. Extracting the cellulose, lignin and ash from the rice husk separately can prevent the influence of other compound components in the rice husk on the performance of the aerated brick, which is beneficial to improve the compressive strength, frost resistance and impermeability of the aerated brick.

[0161] Combining Examples 3-4 and the data in Table 1, it can be seen that when the weight ratio of rice husk ash, rice husk lignin and rice husk filter residue is in the range of (13-14):1:(4-6), the compressive strength and frost resistance of the aerated brick are better, and after multiple freeze-thaw cycles, the compressive strength loss rate and mass loss rate of the aerated brick are lower. This may be because there are still some other compounds in the rice husk filter residue that may affect the gel reaction of the aerated brick slurry, so the amount of rice husk filter residue added is appropriately reduced.

[0162] Combining Examples 4-6 and the data in Table 1, it can be seen that alkali-modified rice husk ash can significantly improve the anti-permeability of aerated bricks, and the compressive strength of aerated bricks is not greatly improved. However, when rice husk ash and alkali-modified rice husk ash are mixed with each other, and the mixing weight ratio is 1: (1.2-1.5), compared with aerated bricks filled with single rice husk ash or single alkali-modified rice husk ash, the mixed filled aerated bricks have better comprehensive performance, with both high compressive strength and good anti-permeability.

[0163] Combining Examples 6-8 and the data in Table 1, it can be seen that if the amount of water reducing agent or water added is kept unchanged, and the rice husk lignin is replaced by the sulfonated modified rice husk lignin, the comprehensive performance of the aerated brick is reduced, while the amount of water reducing agent added is appropriately reduced, and the comprehensive performance of the aerated brick can be restored to the unmodified state and improved, which shows that the sulfonated modified rice husk lignin may have a certain water reducing effect. When the amount of water reducing agent added is appropriately reduced, the aerated bricks with the sulfonated modified rice husk lignin added at this time are compared with the aerated bricks with ordinary rice husk lignin. The former has higher compressive properties and frost resistance. This may be because in a suitable mixing system, the sulfonation modification improves the dispersibility of rice husk lignin in the aerated brick, so that the rice husk lignin can be fully and evenly dispersed in the aerated brick, thereby effectively improving the compressive strength and frost resistance of the aerated brick.

[0164] Combining Examples 8-9 and the data in Table 1, it can be seen that after pretreating the rice husk residue with toluene-2,4-diisocyanate solution, the compressive strength, frost resistance and impermeability of the aerated brick are improved. This may be because the rice husk residue contains rice husk cellulose. When pretreated with toluene-2,4-diisocyanate solution, the toluene-2,4-diisocyanate solution can reduce the hydrophilicity of the rice husk cellulose in the rice husk residue to reduce the agglomeration of the rice husk cellulose itself, so that the pretreated rice husk residue can be fully dispersed in the aerated brick slurry, which greatly reduces the porosity in the aerated brick, and can further improve the compressive strength, frost resistance and impermeability of the aerated brick.

[0165] This specific implementation manner is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make non-creative modifications to the specific implementation manner as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A high-strength environmentally friendly aerated brick, Features: The invention comprises the following raw materials in parts by weight: 15-30 parts of cement; 12-20 parts of quicklime; 20-25 parts of gypsum powder; 80-90 parts of fly ash; 15-30 parts of sand and gravel; 40-60 parts of water; 4-8 parts of aluminum paste; 3-6 parts of coupling agent; Water reducing agent 0.2-0.5 parts; Foam stabilizer 0.7-1.5 parts; 25-65 parts of rice husk extract; The rice husk extract comprises rice husk ash, rice husk lignin and rice husk filter residue, wherein the weight ratio of the rice husk ash, the rice husk lignin and the rice husk filter residue is (13-14):1:(4-6); The extraction method of rice husk ash is: A1. Wash the rice husks with tap water and soak them in water for 10-12 hours, then boil them in HCl solution for 3-4 hours. After boiling, take out the rice husks and dry them; A2, heating the dried rice husk to 500-550°C and calcining for 3-4h to obtain the obtained product; The extraction method of the rice husk lignin and the rice husk residue is: B1. First, grind the rice husk to obtain rice husk powder, then fully mix the rice husk powder, ethanol and an appropriate amount of water, heat to 80-90° C., and stir to react for 3.5-5 hours; B2. After the reaction is completed, the rice husk filtrate and the rice husk residue are separated by filtration, and the rice husk filtrate is evaporated to dryness to obtain rice husk lignin; Specifically, part of the rice husk ash is alkali-modified rice husk ash, and the weight ratio between the rice husk ash and the alkali-modified rice husk ash is 1:(1.2-1.5); the rice husk lignin is sulfonated modified rice husk lignin; the rice husk filter residue is pretreated with a toluene-2,4 diisocyanate solution before mixing, and the toluene-2,4 diisocyanate solution includes toluene-2,4 diisocyanate and a solvent.

2. A high-strength environmentally friendly aerated brick according to claim 1, Features: The preparation method of the alkali-modified rice husk ash is: C1. Mix the rice husk ash with a sodium hydroxide solution having a concentration of 10%-12% in a ratio of 1:(0.8-1), and then keep the reaction at a constant temperature of 80°C-90°C for 5-6 hours, filter the residue to obtain an alkali-modified rice husk ash liquid, and evaporate to dryness to obtain an alkali-modified rice husk ash.

3. A high-strength environmentally friendly aerated brick according to claim 1, Features: The preparation method of the sulfonated modified rice husk lignin comprises: D1. Adding sodium sulfite to the rice husk lignin, heating to 160-180° C., reacting for 1.5-2 hours in an alkaline environment, and obtaining sulfonated modified rice husk lignin.

4. A high-strength environmentally friendly aerated brick according to claim 1, Features: The coupling agent is a mixture of KH550 silane coupling agent and KH560 silane coupling agent, and the weight ratio of the KH550 silane coupling agent to the KH560 silane coupling agent is 1:(2.5-4); The water reducing agent is a polycarboxylic acid water reducing agent, and the foam stabilizer is a silicone resin polyether foam stabilizer.

5. A method for preparing a high-strength environmentally friendly aerated brick according to any one of claims 1 to 4, It is characterized in that The following steps are involved: E1. First, mix cement, quicklime, gypsum powder and fly ash, and grind them into 50-100 mesh cement powder in a ball mill. Then transfer the cement powder to a cement mixing tank, add sand, coupling agent, water reducer, foam stabilizer and rice husk extract, and mix them with the cement powder. Add water and aluminum powder paste, stir evenly to obtain slurry, and then pour the slurry into a mold, wait for the slurry to cool and solidify to obtain the embryo brick; E2. Place the green brick obtained in E1 into a steam curing kettle and evacuate it. Then, introduce steam evenly within 1.8-2 hours to make the temperature in the steam curing kettle reach 170-180 degrees Celsius and the pressure in the kettle reach 1.0-1.2 MPa. Keep the temperature and pressure constant for 9-12 hours. E3. After the reaction is completed, release the steam slowly and evenly. When the temperature in the steam-curing kettle drops to 50°C, take out the brick from the steam-curing kettle and place it at room temperature and pressure for 28-30 days to obtain aerated bricks.