A spray material used in a humid environment and its construction process and application

By optimizing the spraying material of the reaction system of isocyanate group and amino group, the problem of difficult bonding of base materials in humid environment is solved, high hardness and reinforcement effect are achieved, and the cost is reduced. It is suitable for various underground projects, especially large diameters and irregular shapes. Regular pipeline.

CN117659841BActive Publication Date: 2024-10-01WEIFANG FEIMI NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311622510.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-30
Publication Date
2024-10-01
Estimated Expiration
2043-11-30

AI Technical Summary

Technical Problem

Existing spray materials cannot effectively combine with underground pipeline base materials in humid environments, making construction difficult and unable to achieve reinforcement effects. Traditional light-curing materials are costly and cannot be applied to large-diameter and irregular-shaped pipelines.

Method used

Using an optimized reaction system between isocyanate group and amino group and/or hydroxyl group, the prepared spray material contains an isocyanate group compound and a reactive composition, and is sprayed by a high-pressure airless spray machine to form an inner lining with high hardness and high flexural elastic modulus, combined with a catalyst and water-absorbing agents to improve bonding and toughness, avoid shrinkage and cracking, and eliminate the need for primer for construction.

Benefits of technology

It achieves high bonding force and reinforcement effect with the base material in humid environment, reduces construction costs, is suitable for underground projects of various shapes and large diameters, ensures anti-seepage and anti-corrosion performance, and avoids sagging and sagging during construction. Bulging phenomenon.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004579684880000062
    Figure BDA0004579684880000062
  • Figure BDA0004579684880000071
    Figure BDA0004579684880000071
  • Figure BDA0004579684880000081
    Figure BDA0004579684880000081
Patent Text Reader

Abstract

The present invention relates to the technical field of C09D, and specifically to a spray material used in a humid environment, a construction process and an application thereof. The raw materials for preparing the spray material at least include an isocyanate compound and a reactive composition, and the reactive composition at least includes: a compound containing active hydrogen, a catalyst, and a water absorbent, wherein the isocyanate compound has an isocyanate group (NCO) content of 20-32wt%, and the compound containing active hydrogen is selected from an amino compound and / or an alcohol compound. By optimizing the reaction system of the isocyanate group and the amino group and / or the hydroxyl group, the spray material provided has a sufficiently high bonding force with a wet substrate, and at the same time plays a role in reinforcing the substrate, thereby meeting the practical application requirements of trenchless repair of underground pipelines.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of C09D, and in particular to a spraying material used in a humid environment and a construction process and application thereof. Background Art

[0002] During the long-term use of underground pipelines, due to corrosion and scouring, their structural strength decreases, and many of them will leak water, such as sewage pipe leakage. Sewage leaks into the ground and pollutes groundwater, which is also clearly prohibited by the state. If the pipeline is excavated and re-laid with a new pipeline, the excavation will damage the road surface and affect traffic. In some cases, it will affect the use, and even some scenes are very difficult to excavate, such as some key areas, and around shopping malls. Therefore, non-excavation repair of underground pipelines is a very necessary technology. However, during the long-term use of underground pipelines, a large amount of sludge is deposited in the pipelines. During construction, it must be fully cleaned and drained. The pipeline itself has been soaked in water during use. The humidity is 100% after high-pressure water dredging and flushing. It is impossible to dry the pipeline in the underground environment. A basic requirement of traditional anti-corrosion and waterproof materials is that the moisture content of the substrate is below 7%, and the air humidity is below 85%, which cannot be achieved in underground pipelines. If baking is performed, it is very time-consuming and labor-intensive, and the key is that it cannot be completely dried.

[0003] Traditional spray polyurea materials and so-called spray semi-polyurea and spray polyurethane materials on the market are mostly elastomeric waterproof materials. Even for relatively hard spray anti-corrosion polyurethane materials, the substrate moisture content must be below 7% and the air humidity must be below 85% before construction can be carried out. Moreover, most of them need to use matching penetrating primers to obtain good bonding strength, which is obviously impossible to achieve application in humid underground projects. For example, a Chinese patent application (publication number CN111647121 A) discloses a method for preparing a two-component polyurethane composite material for pipeline repair, and a Chinese patent application (authorization announcement number CN109627940B) discloses a polyurea resin composition and a preparation method and construction method thereof. By optimizing the two-component resin and the curing system, the provided material can be used for trenchless repair of underground pipelines. However, it is impossible to have a strong bonding strength and no bulging when the substrate is wet and the environment is humid during construction, while reinforcing the substrate. In addition, the photocuring materials used for trenchless repair of underground pipelines require the substrate to be baked. The bonding strength between the photocuring materials and the substrate is poor, and construction cannot be carried out on large-diameter pipelines (such as pipelines with a diameter of 2 meters) and irregularly shaped underground projects (such as square trenches). In addition, the cost of photocuring materials and construction is high, which limits its practical application. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a spray material for use in a humid environment. By optimizing the reaction system of isocyanate group and amino group and / or hydroxyl group, the provided spray material has a sufficiently high bonding strength with the wet substrate and at the same time plays a role in reinforcing the substrate, thereby meeting the practical application needs of non-excavation repair of underground pipelines.

[0005] On the one hand, the present invention provides a spray material for use in a humid environment, wherein the raw materials for preparing the spray material include at least an isocyanate compound and a reactive composition, wherein the reactive composition includes at least: a compound containing active hydrogen and a water absorbent, wherein the total isocyanate group (NCO) content of the isocyanate compound is 20-32wt%, and the active hydrogen-containing compound is selected from an amino compound and / or an alcohol compound.

[0006] As a preferred technical solution, the volume ratio of the isocyanate compound to the reactive composition is (0.5-1):(0.5-2), preferably 1:1.

[0007] As a preferred technical solution, the isocyanate compound is selected from at least one of polymeric MDI, HDI trimer, HDI biuret, HDI uretdione, semi-prepolymer of MDI-polyol, and semi-prepolymer of polymeric MDI-polyol. Preferably, the semi-prepolymer of MDI-polyol is a semi-prepolymer of MDI-polyether polyol, preferably a semi-prepolymer of MDI-polyether polyol DL1000 or a semi-prepolymer of MDI-polyether polyol DL2000. Preferably, the isocyanate content of the MDI-polyether polyol is 10-15wt%. Preferably, the isocyanate compound is a combination of polymeric MDI and semi-prepolymer of MDI-polyether polyol (isocyanate compound combination A), and the mass ratio of the polymeric MDI and semi-prepolymer of MDI-polyether polyol is (5-9): (1-5). Preferably, the total isocyanate content of the isocyanate compound combination A is 23-29wt%. Further preferably, the isocyanate compound is a combination of polymerized MDI and a semi-prepolymer of MDI-polyether polyol DL1000 (isocyanate compound combination B), the mass ratio of the semi-prepolymer of polymerized MDI and MDI-polyether polyol DL1000 is (7-9):(1-3), the isocyanate group content of the MDI-polyether polyol DL1000 is 10wt%, and the total isocyanate group content of the isocyanate compound combination B is 24.77-29wt%; or the isocyanate compound is a combination of polymerized MDI and a semi-prepolymer of MDI-polyether polyol DL1000 (isocyanate compound combination C), the mass ratio of the semi-prepolymer of polymerized MDI and MDI-polyether polyol DL1000 is 1:1, the isocyanate group content of the MDI-polyether polyol DL2000 is 15wt%, and the total isocyanate group content of the isocyanate compound combination C is 23wt%.

[0008] The spraying material provided by the present invention uses an isocyanate compound with a total isocyanate content of 20-32wt% and a reactive composition containing an amino compound and / or an alcohol compound as raw materials. The polyurethane structure, polyurea structure or a mixture system of polyurethane and polyurea generated by the reaction of the two has a high hard segment content, and the hardness and bending elastic modulus of the cured coating are high. Since most underground pipelines are rough concrete substrates, especially after water sandblasting, silting and grinding, the spraying material is sprayed under high pressure by a two-component high-pressure airless sprayer and penetrates into the substrate, and a continuous and integrated lining repair material with high hardness and high bending elastic modulus is formed on the inner wall of the pipeline. The cured material with high hardness and bending elastic modulus is not easy to fall off from the surface and inside of the substrate, which can ensure that it has a sufficiently high bonding force with the substrate and can also strengthen the substrate.

[0009] Furthermore, based on the requirement of low cost, the spray material is prepared with polymerized MDI as raw material. However, it is found in the actual application process that the spray material shrinks and cracks after construction, and cannot be well applied. During the exploration, the inventor unexpectedly found that the isocyanate compound combination A with a total isocyanate content of 23-29wt% is obtained by combining polymerized MDI and a semi-prepolymer of MDI-polyether polyol DL2000 or MDI-polyether polyol DL1000 with an isocyanate content of 10-15wt% in a mass ratio of (7-9): (1-3). This allows the spray material to effectively reinforce the substrate after construction while ensuring toughness, avoiding shrinkage and cracking, and imparting good anti-corrosion, anti-seepage and reinforcement properties. In addition, the raw material cost is low, and the comprehensive cost is lower than that of photocuring, which is conducive to large-scale promotion and application. This may be due to the appropriate increase in the content of soft segments in the polyurethane and polyurea systems in the coating formed after the reaction with the reactive compositions A and B, which effectively avoids cracking after construction of the spray material while still effectively reinforcing the substrate.

[0010] As a preferred technical solution, the reactive composition comprises at least 0-0.5% of a catalyst, 5-10% of a water absorbent, and the balance is made up of a compound containing active hydrogen, calculated by mass percentage.

[0011] As a preferred technical solution, the active hydrogen-containing compound is selected from at least one of diethyltoluenediamine, 4,4'-methylenebis(2-chloroaniline), dimethylthiotoluenediamine, polyetheramine, castor oil-based polyol, polyoxypropylene ether polyol, and polyaspartic acid ester resin. Preferably, the molecular weight (average molecular weight or relative molecular weight) of the polyetheramine and polyaspartic acid ester resin is ≤1000, and the functionality of the castor oil-based polyol and polyoxypropylene ether polyol is 2.5-4, and the molecular weight (average molecular weight or relative molecular weight) is 200-1000. Preferably, the active hydrogen-containing compound is selected from diethyltoluenediamine (E100), 4,4'-methylenebis(2-chloroaniline) (MOCA), dimethylthiotoluenediamine (E300), polyetheramine T403, polyetheramine D230, polyoxypropylene ether polyol TMN450, polyoxypropylene ether polyol TMN700, 750, 908, polycin M-365, polyaspartic acid resin F420, polyaspartic acid resin F524, polyaspartic acid resin F220. Preferably, the active hydrogen-containing compound is diethyltoluenediamine (E100), polyetheramine T403, 750 (reactive composition A) or polycin M-365 and polyaspartic acid ester resin F524 (reactive composition B).

[0012] Preferably, the diethyltoluenediamine, polyetheramine T403, The mass ratio of polycin M-365 and polyaspartic acid resin F524 is (80-85): (15-20), preferably 83.6:11.4.

[0013] Further, based on the isocyanate compound combination B or the isocyanate compound combination C used in the present invention, diethyltoluenediamine, polyetheramine T403, 750 (reactive composition A) or a combination of polycin M-365 and polyaspartic acid ester resin F524 in a mass ratio of (80-85): (15-20) (reactive composition B) is used together, and no primer is required to achieve strong bonding and no bulging when the substrate is wet and the environment is humid. At the same time, the sustainable spraying performance (recoating performance) of the spraying material is guaranteed, the sagging phenomenon during construction is avoided, and the actual application needs of non-excavation repair of underground pipelines are better met. This may be because the gel reaction speed of the reactive composition A and the reactive composition B after being matched with the isocyanate compound combination B or the isocyanate compound combination C is faster than the reaction speed of isocyanate and water, thereby avoiding the bulging and decreased adhesion caused by the foaming of the main material and ensuring the gel speed to achieve continuous spraying and ensure the interlayer bonding strength. At this time, the main material is a polyurethane-polyurea composite structure system, and the hard segment content in the system is increased, the chain segment movement is difficult, and the phase separation degree is low. Therefore, no primer is required to achieve strong bonding when the substrate is wet and the environment is wet. At the same time, the sustainable spraying performance (recoating performance) of the spraying material is guaranteed, and the sagging phenomenon during construction is avoided, so as to better meet the actual application needs of trenchless repair of underground pipelines.

[0014] As a preferred technical solution, the catalyst is catalyst CUCAT-HA02 and / or catalyst CUCAT-HA01, preferably catalyst CUCAT-HA02 (Guangzhou Yourun Synthetic Materials Co., Ltd.).

[0015] As a preferred technical solution, the water absorbent is a molecular sieve, and the molecular sieve is preferably molecular sieve A3 powder.

[0016] As a preferred technical solution, the volume ratio of the isocyanate compound combination B or C to the reactive composition is 1:1, and the mass ratio of the reactive composition A or B, the catalyst CUCAT-HA02, and the molecular sieve A3 powder is (90-95):0.5:(5-10), preferably 95:0.5:5.

[0017] The spray material system provided by the present invention further ensures the compactness of the spray material after construction by introducing the catalyst CUCAT-HA02 and the molecular sieve A3 powder into the reactive composition and further controlling the addition amount of the two, and ensures the application performance of the spray material after construction under the working conditions of the substrate being wet and the environment being wet, thereby providing a new technical solution for the application of underground engineering. The inventors analyzed that the reason may be that under the joint action of the above-mentioned addition amount of CUCAT-HA02 and the molecular sieve A3 powder, the polycin M-365 or 750 reacts specifically with the isocyanate group in the isocyanate compound combination B or C, avoiding the foaming and bulging problems caused by the reaction of water and isocyanate groups in a moist substrate or moist environment to the greatest extent, and obtaining a soft and hard segmented polyurethane structure, and a polyurea structure obtained by the reaction of the isocyanate compound combination B or C with diethyltoluenediamine, polyetheramine T403 or polyaspartic acid ester resin F524, to ensure the density of the spray material after construction.

[0018] Another aspect of the present invention provides a spray material construction process for use in a humid environment, comprising at least the following steps:

[0019] (1) The substrate is cleaned after grinding or dredged by high-pressure water washing or water sandblasting to make the substrate surface rough;

[0020] (2) Drain and clean the clear water;

[0021] (3) Using spraying equipment to spray the spray material onto the surface of the substrate.

[0022] As a preferred technical solution, the spraying equipment is a two-component high-pressure airless sprayer.

[0023] The spray material provided by the present invention can be used for underground projects of any shape, such as pipelines, square trenches, integrated pipe galleries, etc., by matching the above-mentioned spray construction process, and can also achieve anti-seepage and anti-corrosion construction for large-diameter pipelines such as 2 meters. There are already a large number of successful application cases (such as: the urban pipeline reconstruction and expansion project in Yangli District, Fuzhou City, the underground project of Fuchengmennei Street in Beijing, the inner wall application of underground pipelines on West Fourth Ring Road South Road in Fengtai District, Beijing, and the inner wall application of underground pipelines at the southwest corner of Fuchengmen Bridge on West Second Ring Road in Beijing, etc.).

[0024] Beneficial Effects

[0025] 1. The present invention provides a spray material for use in a humid environment. By optimizing the reaction system of isocyanate groups and amino and / or hydroxyl groups, the provided spray material has a sufficiently high bonding strength with the wet substrate and at the same time plays a role in reinforcing the substrate, thereby meeting the practical application needs of trenchless repair of underground pipelines.

[0026] 2. The spray material provided by the present invention uses an isocyanate compound with a total isocyanate content of 20-32wt% and a reactive composition containing an amino compound and / or an alcohol compound as raw materials. After construction, a continuous and integrated lining repair material with high hardness and high bending elastic modulus is formed on the inner wall of the pipeline. The cured material with high hardness and bending elastic modulus is not easy to fall off from the surface and interior of the substrate, which can ensure a sufficiently high bonding force with the substrate and can also reinforce the substrate.

[0027] 3. The present invention obtains an isocyanate compound combination A with a total isocyanate content of 23-29 wt% by combining polymerized MDI and a semi-prepolymer of MDI-polyether polyol DL2000 or MDI-polyether polyol DL1000 with an isocyanate content of 10-15 wt% in a mass ratio of (7-9): (1-3). After the spraying material is applied, the base material is effectively reinforced while ensuring toughness and avoiding shrinkage cracking, thereby imparting good anti-corrosion, anti-seepage and reinforcement properties. The raw material cost is low, and the overall cost is lower than that of photocuring, which is conducive to large-scale promotion and application.

[0028] 4. Based on the isocyanate compound combination B or the isocyanate compound combination C used in the present invention, diethyltoluenediamine, polyetheramine T403, 750 (reactive composition A) or a combination of polycin M-365 and polyaspartic acid ester resin F524 in a mass ratio of (80-85): (15-20) (reactive composition B) is used together, and no primer is required to achieve strong bonding and no bulging when the substrate is wet and the environment is humid. At the same time, the sustainable spraying performance (recoating performance) of the spraying material is guaranteed, the sagging phenomenon during construction is avoided, and the actual application needs of non-excavation repair of underground pipelines are better met.

[0029] 5. The spray material provided by the present invention can be used for underground projects of any shape, such as pipelines, square trenches, integrated pipe galleries, etc., by matching the spray construction process, and can also achieve anti-seepage and anti-corrosion construction for large-diameter pipelines such as 2 meters. DETAILED DESCRIPTION

[0030] Example 1

[0031] Embodiments 1-10 of the present invention provide a spray material for use in a humid environment, and the raw materials for preparing the spray material are shown in Table 1.

[0032] Table 1

[0033]

[0034]

[0035]

[0036] On the other hand, embodiments 1-10 of the present invention provide a method for preparing a spray material for use in a humid environment, comprising the following steps:

[0037] (1) sandblasting the substrate with water to make the surface of the substrate rough;

[0038] (2) Drain and clean the clear water;

[0039] (3) Using spraying equipment to spray the spray material onto the surface of the substrate.

[0040] The spraying equipment is a two-component high-pressure airless sprayer.

[0041] Performance Testing Methods

[0042] (1) Gel time, s, refer to GB / T23446-2009 spray polyurea waterproof coating, the results are shown in Table 2.

[0043] (2) Tensile strength, MPa, tested according to GB / T2567-2008 resin casting performance test method, the results are shown in Table 2.

[0044] (3) Hardness, Shore D: The indentation hardness was measured using a durometer according to GB / T 2411-2008 for plastics and hard rubber. The results are shown in Table 2.

[0045] (4) Compressive strength, MPa, tested according to GB / T2567-2008 resin casting performance test method, the results are shown in Table 2.

[0046] (5) Flexural strength, MPa, tested according to GB / T2567-2008 resin casting performance test method, the results are shown in Table 2.

[0047] (6) Flexural modulus, MPa, tested according to GB / T2567-2008 resin casting performance test method, the results are shown in Table 2.

[0048] (7) Adhesion, MPa, tested according to GB / T16777-2008 test method for building waterproof coatings. The results are shown in Table 2.

[0049] Table 2

[0050]

[0051]

Claims

1. A spray material used in a humid environment, characterized in that: The preparation raw materials at least include an isocyanate compound and a reactive composition, and the reactive composition at least includes: an active hydrogen-containing compound and a water absorbent, wherein the total isocyanate content of the isocyanate compound is 20-32wt%, the isocyanate compound is a combination of polymerized MDI and a semi-prepolymer of MDI-polyether polyol, the mass ratio of the polymerized MDI and the semi-prepolymer of MDI-polyether polyol is (5-9): (1-5), the semi-prepolymer of MDI-polyol is a semi-prepolymer of MDI-polyether polyol, and the isocyanate content of the MDI-polyether polyol is 10-15wt%; the active hydrogen-containing compound is a combination of diethyltoluenediamine, polyetheramine T403, and Sofumoer® 750 or a combination of polycin M-365 and polyaspartic acid ester resin F524; the diethyltoluenediamine, polyetheramine T403, Sofumoer® The mass ratio of 750 is (5-11): (9.5-20): (64.5-80); the mass ratio of polycinM-365 and polyaspartic acid ester resin F524 is (80-85): (15-20); the volume ratio of the isocyanate compound and the reactive composition is (0.5-1): (0.5-2).

2. The spray material for use in a humid environment according to claim 1, characterized in that: Calculated by mass percentage, the reactive composition at least includes 0-0.5% of a catalyst, 5-10% of a water absorbent, and the balance is made up of a compound containing active hydrogen.

3. A construction process for a spray material used in a humid environment according to any one of claims 1-2, characterized in that: At least the following steps are included: (1) Grind and clean the substrate or use high-pressure water washing or water sandblasting to make the substrate surface rough; (2) Drain and clean the surface water; (3) Use spraying equipment to spray the spray material onto the surface of the substrate.