A processing method of high-strength composite resin for air duct processing

The resin material for air ducts is solved by combining the resin reinforcement modified with modified polysiloxane and 9,10-dihydro-9-oxa-10-phosphazepamphene-10-oxide and the matrix resin. The problem of insufficient mechanical properties and corrosion resistance has achieved improvements in high strength, high temperature resistance and flame retardant properties.

CN117683252BActive Publication Date: 2024-11-05SHENZHEN DAYI NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311743132.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-18
Publication Date
2024-11-05
Estimated Expiration
2043-12-18

AI Technical Summary

Technical Problem

The mechanical properties and mechanical strength of the resin material for air ducts need to be improved, and it is easily corroded or damaged in corrosive chemical substances such as acids, alkalis, solvents or high-temperature flue gases, and the corrosion resistance and high-temperature resistance are insufficient.

Method used

The resin reinforcement modified with modified polysiloxane, 9,10-dihydro-9-oxa-10-phosphazepamphene-10-oxide and the matrix resin are combined, through silicone bonds and olefin bis The intermolecular forces and chemical crosslinking of functional groups such as bonds and benzene rings improve the compatibility and crosslinking of resins and fibers, and enhance the mechanical properties and corrosion resistance of materials.

Benefits of technology

It significantly improves the mechanical properties, corrosion resistance and flame retardant properties of composite resins, extends service life, and maintains good mechanical properties and light transmittance in high-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004613715150000021
    Figure BDA0004613715150000021
  • Figure BDA0004613715150000031
    Figure BDA0004613715150000031
  • Figure BDA0004613715150000041
    Figure BDA0004613715150000041
Patent Text Reader

Abstract

The invention discloses a processing method of a high-strength composite resin for wind tube processing, and belongs to the technical field of resin processing. The invention is used to solve the technical problem that the mechanical properties, mechanical strength, corrosion resistance and high temperature resistance of the resin material for wind tube in the prior art need to be further improved. A processing method of a high-strength composite resin for wind tube processing comprises the following steps: adding modified polysiloxane and acetone to a nitrogen-protected three-necked flask and stirring, slowly dropping 3-isocyanate propylene into the three-necked flask, and after the dropwise addition is completed, the temperature of the three-necked flask is raised to 40-50°C, and the reaction is kept warm for 2-3h to obtain an intermediate I. The present invention prepares a composite resin material with good compatibility and high crosslinking degree by using reinforcing fiber and resin reinforcing agent to cooperate with matrix resin, which not only effectively improves the bending performance and impact resistance of the composite resin, but also improves the high temperature resistance, corrosion resistance and combustion grade of the composite resin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of resin processing, and in particular to a processing method of high-strength composite resin for air duct processing. Background Art

[0002] With the development of modern industry, the demand for high-strength composite materials is increasing. High-strength composite materials have the advantages of light weight, high strength, and good corrosion resistance. They are widely used in aerospace, automobile, shipbuilding and other fields. In the field of air duct processing, metal materials such as aluminum alloys are mostly used to manufacture air ducts. However, there are some shortcomings of metal materials. First, metal materials are relatively heavy and susceptible to corrosion. Secondly, the process of metal materials is complicated, requiring high energy consumption and professional technology. In addition, metal materials are prone to fatigue during the stress process, which reduces the service life of the air duct and increases maintenance costs. Traditional metal materials are gradually replaced by high-strength composite resins to improve lightweight effects and durability.

[0003] Existing resin materials for air ducts usually use high-temperature resistant resin raw materials in combination with fiber-reinforced materials such as glass fiber and carbon fiber to improve the mechanical strength of the resin material. However, there is a large difference in polarity between the resin and the fiber-reinforced material, and the degree of cross-linking between the fiber-reinforced material and the resin is poor. The mechanical properties and mechanical strength of the resin material for air ducts need to be further improved. In addition, air ducts are usually used in some special industrial environments, where corrosive chemicals such as acids, alkalis, and solvents or high-temperature flue gases may exist, causing the air duct to be corroded or damaged by high temperature. The corrosion resistance and high-temperature resistance of the resin material for air ducts need to be further improved.

[0004] In view of the technical defects in this aspect, a solution is now proposed. Summary of the invention

[0005] The purpose of the present invention is to provide a processing method for high-strength composite resin for air duct processing, which is used to solve the technical problems in the prior art that the resin material for the air duct, the degree of crosslinking between the fiber reinforced material and the resin is poor, the mechanical properties and mechanical strength of the resin material for the air duct need to be further improved, the air duct is easily corroded or damaged by corrosive chemicals such as acids, alkalis, solvents or high-temperature flue gases, and the corrosion resistance and high-temperature resistance of the resin material for the air duct need to be further improved.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A method for processing a high-strength composite resin for processing an air duct comprises the following steps:

[0008] S1. Add modified polysiloxane and acetone into a three-necked flask protected by nitrogen and stir, slowly drop 3-isocyanate propylene into the three-necked flask, and after the dropwise addition is completed, raise the temperature of the three-necked flask to 40-50° C. and keep the temperature for 2-3 hours to obtain intermediate I;

[0009] The synthetic reaction principle of intermediate I is:

[0010]

[0011] S2, adding intermediate I, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, n-propanol and a catalyst into a three-necked flask and stirring, raising the temperature of the three-necked flask to 75-85° C., keeping the temperature for reaction for 8-10 hours, and post-treating to obtain intermediate II;

[0012] The synthetic reaction principle of intermediate II is:

[0013]

[0014] S3, adding intermediate II and acetone into a three-necked flask protected by nitrogen and stirring, slowly adding isocyanatepropyltriethoxysilane into the three-necked flask, raising the temperature of the three-necked flask to 45-50° C., keeping the temperature for reaction for 6-8 hours, and post-treating to obtain a resin reinforcing agent;

[0015] The synthetic reaction principle of resin enhancer is:

[0016]

[0017] S4. Add the base resin and acetone into a beaker, heat and stir until the system is dissolved, add the reinforcing fiber and resin reinforcing agent into the beaker, stir evenly, and after vacuum degassing, add it into the mold to cool and shape, demold, and obtain the composite resin.

[0018] Furthermore, in step S1, the amount ratio of modified polysiloxane, acetone and 3-isocyanate propylene is 6g:18mL:1g, and the post-processing operation includes: after the reaction is completed, the temperature of the three-necked flask is kept at 40-50°C, and the solvent is evaporated under reduced pressure to obtain intermediate I; in step S2, the amount ratio of intermediate I, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, n-propanol and catalyst is 10g:0.6g:30mL:0.1g, and the catalyst is azobisisobutyronitrile, and the post-processing operation includes: after the reaction is completed, the three-necked flask is kept at 75-85°C, and the solvent is evaporated under reduced pressure to obtain intermediate II; in step S3, the amount ratio of intermediate II, acetone and isocyanatepropyltriethoxysilane is 3g:10mL:1g, and the post-processing operation includes: after the reaction is completed, the solvent is evaporated under reduced pressure to obtain a resin reinforcing agent.

[0019] Further, the modified polysiloxane is processed by the following steps:

[0020] A1. Add methyldiethoxysilane, dimethyldiethoxysilane and anhydrous ethanol into a three-necked flask and stir. Add 10 wt % sodium hydroxide solution into the three-necked flask. Raise the temperature of the three-necked flask to a micro-reflux state. Keep the temperature for 6-8 hours and perform post-treatment to obtain polysiloxane.

[0021] The synthetic reaction principle of polysiloxane is:

[0022]

[0023] A2. Add polysiloxane, propylene alcohol and catalyst into a three-necked flask and stir. Raise the temperature of the three-necked flask to 80-90° C. and keep the temperature to react for 4-6 hours. Post-treat to obtain modified polysiloxane.

[0024] The synthetic reaction principle of modified polysiloxane is:

[0025]

[0026] Furthermore, in step A1, the dosage ratio of methyldiethoxysilane and dimethyldiethoxysilane is 5mol:3mol, the dosage ratio of dimethyldiethoxysilane, anhydrous ethanol and 10wt% sodium hydroxide is 1g:5mL:2mL, and the post-treatment operation includes: after the reaction is completed, the temperature of the three-necked flask is reduced to room temperature, hydrochloric acid is added to the three-necked flask, the pH of the system is adjusted to 7, the temperature of the three-necked flask is increased to 70-80°C, the solvent is evaporated under reduced pressure, anhydrous ethanol is added to the three-necked flask, suction is filtered, and the filtrate is transferred to a rotary evaporator, and the water bath temperature is set to 55-65°C to evaporate ethanol under reduced pressure to obtain polysiloxane.

[0027] Furthermore, in step A2, the weight ratio of polysiloxane, acryl alcohol and catalyst is 6:1:0.3, the catalyst is 10wt% chloroplatinic acid / isopropanol solution, and the post-treatment operation includes: after the reaction is completed, the temperature of the three-necked flask is increased to 90-100°C, and the reduced pressure distillation is performed until no liquid flows out to obtain modified polysiloxane.

[0028] Furthermore, the preparation method of the matrix resin is as follows: 4,4'-di(methoxymethyl)diphenyl ether, phenol, and a catalyst are added to a three-necked flask and stirred, the temperature of the three-necked flask is increased to 120-130°C, the pressure is reduced to -0.1MPa, and the reaction is kept warm for 2-3h, the temperature of the three-necked flask is reduced to 80-90°C, polyformaldehyde is added to the three-necked flask, the pressure of the three-necked flask is reduced to -0.1MPa, and the reaction is kept warm for 2-3h to obtain the matrix resin.

[0029] The synthetic reaction principle of the matrix resin is:

[0030]

[0031] Furthermore, the usage ratio of the 4,4'-bis(methoxymethyl)diphenyl ether and phenol is 1 mol:2 mol, the weight ratio of the phenol, the catalyst and polyoxymethylene is 10:0.1:11, and the catalyst is sodium hydroxide.

[0032] Furthermore, in step S4, the weight ratio of the matrix resin, acetone, reinforcing fiber and resin reinforcing agent is 10:15:5:7, and the reinforcing fiber is one or more of glass fiber, polyester fiber, polypropylene fiber, carbon fiber and aramid fiber.

[0033] The present invention has the following beneficial effects:

[0034] 1. The composite resin of the present invention is compounded with a resin reinforcing agent containing a large number of siloxane bonds, olefin double bonds and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide modified polysiloxane long chains and a matrix resin containing a large number of benzene rings and hydroxyl modifications. The molecules of functional groups such as hydroxyl groups, ether bonds and carbon-carbon double bonds in the matrix resin can generate intermolecular or intramolecular forces with the siloxane bonds and olefin double bonds in the resin reinforcing agent, thereby improving the compatibility between the resin reinforcing agent and the matrix resin, and the siloxane bonds on the resin reinforcing agent can chemically crosslink with the active groups on the matrix resin or the reinforcing fibers, thereby improving the compatibility between the matrix resin and the reinforcing fibers in the composite resin, and then effectively improving the crosslinking degree of the composite resin, thereby improving the mechanical properties and corrosion resistance of the composite resin material, and the 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide cooperates with siloxane to further improve the flame retardant properties of the composite resin material.

[0035] 2. In the preparation process of the composite resin of the present invention, 4,4'-bis(methoxymethyl)diphenyl ether and phenol are subjected to an ether exchange reaction in an alkaline environment, and then the hydroxyl group on the phenol reacts with the ether bond of the 4,4'-bis(methoxymethyl)diphenyl ether and then undergoes an addition polycondensation reaction with polyformaldehyde to prepare a matrix resin. By introducing a large number of benzene rings into the matrix resin, the high temperature resistance of the matrix resin is improved, and the polyformaldehyde and the easily oxidizable phenolic hydroxyl structure on the phenol form alcoholic hydroxyl groups in the matrix resin, thereby improving the reactivity of the matrix resin. The siloxane bonds on the resin reinforcing agent are easily broken in a high temperature environment to form silanol groups, which can react with the matrix resin or the surface active matrix of the reinforcing fiber to form chemical crosslinks, thereby improving the crosslinking degree between the reinforcing fiber and the matrix resin in the composite resin, thereby effectively improving the mechanical strength of the composite resin material.

[0036] 3. In the preparation process of the composite resin of the present invention, methyldiethoxysilane and dimethyldiethoxysilane are used as raw materials, and a self-assembly reaction is performed after hydrolysis in an alkaline environment. By controlling the composition ratio of the raw materials, a polysiloxane having a long straight chain and containing a large amount of active hydrogen on silicon is generated. Under the action of a catalyst, the active hydrogen on the oily polysiloxane undergoes a substitution addition reaction with allyl alcohol to form a modified polysiloxane with a large amount of hydroxyl groups grafted on the molecular chain, which effectively improves the reactivity of the polysiloxane. The hydroxyl groups on the modified polysiloxane undergo a condensation reaction with 3-isocyanate propylene. After the olefin double bond modification is formed on the modified polysiloxane chain segment, a substitution addition reaction occurs with 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide under the action of a catalyst to form an intermediate II. The active hydroxyl group on the intermediate II reacts with isocyanatepropyltriethoxysilane to form a resin reinforcing agent containing a large number of siloxane bonds, olefin double bonds and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide modified polysiloxane long chains, thereby improving the intermolecular force between the resin reinforcing agent and the matrix resin and the crosslinking density of the composite resin, thereby improving its heat resistance and Chemical stability, while maintaining good mechanical properties and light transmittance, siloxane can also form a dense protective film on the resin surface to prevent the penetration of moisture, oxygen and corrosive substances, thereby further enhancing the corrosion resistance of the resin; 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is modified on the resin reinforcing agent in the form of chemical cross-linking, and is evenly dispersed in the composite resin along with the resin reinforcing agent, which effectively improves the dispersibility of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide in the composite resin, and 9,10-dihydro-9-oxa- 10-Phosphophenanthrene-10-oxide can form coordination bonds with silicon atoms in siloxane through the oxygen atoms in its structure, thereby effectively combining 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide with siloxane, increasing the thermal stability and flame retardancy of the composite material while maintaining good mechanical properties and light transmittance. 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide can also copolymerize with the olefin double bonds in siloxane, thereby significantly improving the flame retardancy and thermal stability of the material while maintaining the good mechanical properties of the composite resin. DETAILED DESCRIPTION

[0037] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] Example 1

[0039] This embodiment provides a method for processing a high-strength composite resin for processing a wind tube, comprising the following steps:

[0040] S1. Preparation of base resin

[0041] Weigh: 25.8 g of 4,4'-bis(methoxymethyl)diphenyl ether, 18.8 g of phenol, and 0.2 g of sodium hydroxide, add into a three-necked flask and stir, raise the temperature of the three-necked flask to 120°C, reduce the pressure to -0.1 MPa, and keep warm for 2 hours, lower the temperature of the three-necked flask to 80°C, add 20.7 g of polyformaldehyde into the three-necked flask, reduce the pressure of the three-necked flask to -0.1 MPa, and keep warm for 2 hours to obtain a matrix resin.

[0042] S2. Preparation of modified polysiloxane

[0043] Weigh: 67.1 g of methyldiethoxysilane, 44.5 g of dimethyldiethoxysilane, and 222.5 mL of anhydrous ethanol, add them to a three-necked flask and stir, add 89 mL of a 10 wt% sodium hydroxide solution to the three-necked flask, raise the temperature of the three-necked flask to a micro-reflux of the system, keep the temperature for 6 hours, lower the temperature of the three-necked flask to room temperature, add hydrochloric acid to the three-necked flask, adjust the pH of the system to 7, raise the temperature of the three-necked flask to 70° C., evaporate the solvent under reduced pressure, add anhydrous ethanol to the three-necked flask, filter, transfer the filtrate to a rotary evaporator, set the water bath temperature to 55° C., evaporate the ethanol under reduced pressure, and obtain polysiloxane;

[0044] Weigh: 60 g of polysiloxane, 10 g of allyl alcohol and 3 g of 10 wt% chloroplatinic acid / isopropanol solution, add into a three-necked flask and stir, raise the temperature of the three-necked flask to 80° C., keep warm and react for 4 hours, raise the temperature of the three-necked flask to 90° C., and distill under reduced pressure until no liquid flows out to obtain modified polysiloxane.

[0045] S3. Preparation of resin reinforcing agent

[0046] Weigh: 60 g of modified polysiloxane and 180 mL of acetone are added to a three-necked flask protected by nitrogen and stirred. 10 g of 3-isocyanate propylene is slowly added dropwise to the three-necked flask. After the addition is completed, the temperature of the three-necked flask is raised to 40° C. and the reaction is kept warm for 2 h. The temperature of the three-necked flask is kept at 40° C. and the solvent is evaporated under reduced pressure to obtain intermediate I;

[0047] Weigh: 60 g of intermediate I, 3.6 g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 180 mL of n-propanol and 0.6 g of azobisisobutyronitrile, add into a three-necked flask and stir, raise the temperature of the three-necked flask to 75° C., keep warm for 8-10 hours, keep the three-necked flask at 75° C., and evaporate the solvent under reduced pressure to obtain intermediate II;

[0048] Weigh: 60 g of intermediate II and 200 mL of acetone are added into a three-necked flask protected by nitrogen and stirred. 20 g of isocyanatepropyltriethoxysilane is slowly added into the three-necked flask. The temperature of the three-necked flask is raised to 45° C. and the reaction is kept warm for 6 hours. The solvent is evaporated under reduced pressure to obtain a resin reinforcing agent.

[0049] S4. Preparation of composite resin

[0050] Weigh: 500g of base resin and 750g of acetone are added to a beaker, heated and stirred until the system is dissolved, 150g of glass fiber, 100g of polypropylene fiber and 350g of resin reinforcing agent are added to the beaker, stirred evenly, and after vacuum degassing, added to the mold to cool and shape, demold, and obtain composite resin.

[0051] Example 2

[0052] This embodiment provides a method for processing a high-strength composite resin for processing a wind tube, comprising the following steps:

[0053] S1. Preparation of base resin

[0054] Weigh: 25.8 g of 4,4'-bis(methoxymethyl)diphenyl ether, 18.8 g of phenol, and 0.2 g of sodium hydroxide, add into a three-necked flask and stir, raise the temperature of the three-necked flask to 125°C, reduce the pressure to -0.1 MPa, and keep warm for 2.5 hours. Lower the temperature of the three-necked flask to 85°C, add 20.7 g of polyformaldehyde into the three-necked flask, reduce the pressure of the three-necked flask to -0.1 MPa, and keep warm for 2.5 hours to obtain a matrix resin.

[0055] S2. Preparation of modified polysiloxane

[0056] Weigh: 67.1 g of methyldiethoxysilane, 44.5 g of dimethyldiethoxysilane, and 222.5 mL of anhydrous ethanol, add them to a three-necked flask and stir, add 89 mL of a 10 wt% sodium hydroxide solution to the three-necked flask, raise the temperature of the three-necked flask to a micro-reflux of the system, keep the reaction warm for 7 hours, lower the temperature of the three-necked flask to room temperature, add hydrochloric acid to the three-necked flask, adjust the pH of the system to 7, raise the temperature of the three-necked flask to 75° C., evaporate the solvent under reduced pressure, add anhydrous ethanol to the three-necked flask, filter, transfer the filtrate to a rotary evaporator, set the water bath temperature to 60° C., evaporate the ethanol under reduced pressure, and obtain polysiloxane;

[0057] Weigh: 60 g of polysiloxane, 10 g of allyl alcohol and 3 g of 10 wt% chloroplatinic acid / isopropanol solution, add into a three-necked flask and stir, raise the temperature of the three-necked flask to 85° C., keep warm and react for 5 hours, raise the temperature of the three-necked flask to 95° C., and distill under reduced pressure until no liquid flows out to obtain modified polysiloxane.

[0058] S3. Preparation of resin reinforcing agent

[0059] Weigh: 60 g of modified polysiloxane and 180 mL of acetone are added to a three-necked flask protected by nitrogen and stirred. 10 g of 3-isocyanate propylene is slowly added dropwise to the three-necked flask. After the addition is completed, the temperature of the three-necked flask is raised to 43° C. and the reaction is kept warm for 2.5 hours. The temperature of the three-necked flask is kept at 45° C. and the solvent is evaporated under reduced pressure to obtain intermediate I;

[0060] Weigh: 60 g of intermediate I, 3.6 g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 180 mL of n-propanol and 0.6 g of azobisisobutyronitrile, add into a three-necked flask and stir, raise the temperature of the three-necked flask to 80° C., keep the temperature for 9 h, keep the three-necked flask at 80° C., and evaporate the solvent under reduced pressure to obtain intermediate II;

[0061] Weigh: 60 g of intermediate II and 200 mL of acetone are added into a three-necked flask protected by nitrogen and stirred. 20 g of isocyanatepropyltriethoxysilane is slowly added into the three-necked flask. The temperature of the three-necked flask is raised to 47° C. and the reaction is kept warm for 7 hours. The solvent is evaporated under reduced pressure to obtain a resin reinforcing agent.

[0062] S4. Preparation of composite resin

[0063] Weigh: 500g of base resin and 750g of acetone are added to a beaker, heated and stirred until the system is dissolved, 150g of glass fiber, 100g of polyester fiber and 350g of resin reinforcing agent are added to the beaker, stirred evenly, and after vacuum degassing, added to the mold to cool and shape, demold, and obtain composite resin.

[0064] Example 3

[0065] This embodiment provides a method for processing a high-strength composite resin for processing a wind tube, comprising the following steps:

[0066] S1. Preparation of base resin

[0067] Weigh: 25.8 g of 4,4'-bis(methoxymethyl)diphenyl ether, 18.8 g of phenol, and 0.2 g of sodium hydroxide, add into a three-necked flask and stir, raise the temperature of the three-necked flask to 120-130°C, reduce the pressure to -0.1 MPa, and keep warm for 3 hours, lower the temperature of the three-necked flask to 90°C, add 20.7 g of polyformaldehyde into the three-necked flask, reduce the pressure of the three-necked flask to -0.1 MPa, and keep warm for 3 hours to obtain a matrix resin.

[0068] S2. Preparation of modified polysiloxane

[0069] Weigh: 67.1 g of methyldiethoxysilane, 44.5 g of dimethyldiethoxysilane, and 222.5 mL of anhydrous ethanol, add them to a three-necked flask and stir, add 89 mL of a 10 wt% sodium hydroxide solution to the three-necked flask, raise the temperature of the three-necked flask to a micro-reflux of the system, keep the temperature for reaction for 8 hours, lower the temperature of the three-necked flask to room temperature, add hydrochloric acid to the three-necked flask, adjust the pH of the system to 7, raise the temperature of the three-necked flask to 80° C., evaporate the solvent under reduced pressure, add anhydrous ethanol to the three-necked flask, filter, transfer the filtrate to a rotary evaporator, set the water bath temperature to 65° C., evaporate the ethanol under reduced pressure, and obtain polysiloxane;

[0070] Weigh: 60 g of polysiloxane, 10 g of allyl alcohol and 3 g of 10 wt% chloroplatinic acid / isopropanol solution, add into a three-necked flask and stir, raise the temperature of the three-necked flask to 90° C., keep warm and react for 6 hours, raise the temperature of the three-necked flask to 100° C., and distill under reduced pressure until no liquid flows out to obtain modified polysiloxane.

[0071] S3. Preparation of resin reinforcing agent

[0072] Weigh: 60 g of modified polysiloxane and 180 mL of acetone are added to a three-necked flask protected by nitrogen and stirred. 10 g of 3-isocyanate propylene is slowly added dropwise to the three-necked flask. After the addition is completed, the temperature of the three-necked flask is raised to 50° C. and the reaction is kept at this temperature for 3 h. The temperature of the three-necked flask is kept at 50° C. and the solvent is evaporated under reduced pressure to obtain intermediate I;

[0073] Weigh: 60 g of intermediate I, 3.6 g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 180 mL of n-propanol and 0.6 g of azobisisobutyronitrile, add into a three-necked flask and stir, raise the temperature of the three-necked flask to 85° C., keep the temperature for 10 h, keep the three-necked flask at 85° C., and evaporate the solvent under reduced pressure to obtain intermediate II;

[0074] Weigh: 60 g of intermediate II and 200 mL of acetone are added into a three-necked flask protected by nitrogen and stirred. 20 g of isocyanatepropyltriethoxysilane is slowly added into the three-necked flask. The temperature of the three-necked flask is raised to 50° C. and the reaction is kept warm for 8 hours. The solvent is evaporated under reduced pressure to obtain a resin reinforcing agent.

[0075] S4. Preparation of composite resin

[0076] Weigh: 500g of base resin and 750g of acetone are added to a beaker, heated and stirred until the system is dissolved, 150g of glass fiber, 100g of aramid fiber and 350g of resin reinforcing agent are added to the beaker, stirred evenly, and after vacuum degassing, added to the mold to cool and shape, demold, and obtain composite resin.

[0077] Comparative Example 1

[0078] The difference between this comparative example and Example 3 is that step S3 is eliminated, and the reinforcing resin in step S4 is replaced by an equal amount of the modified polysiloxane obtained in step S2.

[0079] Comparative Example 2

[0080] The difference between this comparative example and Example 3 is that in step S3, an equal amount of modified polysiloxane is used to replace the intermediate II in the reaction of preparing the resin reinforcing agent.

[0081] Comparative Example 3

[0082] The difference between this comparative example and Example 3 is that the resin reinforcing agent in step S4 is replaced by an equal amount of the intermediate II in step S3.

[0083] Comparative Example 4

[0084] The difference between this comparative example and Example 3 is that no resin reinforcing agent is added in step S4.

[0085] Performance Test:

[0086] The strength, high temperature resistance, corrosion resistance and wear resistance of the composite resins prepared in Examples 1-3 and Comparative Examples 1-3 were tested. The strength was measured by referring to the standards GB / T 1449-2005 "Fiber reinforced plastic bending properties test method" and GB / T1451-2005 "Fiber reinforced plastic simply supported beam impact toughness test method" to determine the bending strength, breaking deflection and impact toughness of the sample; the high temperature resistance was measured by referring to the standard GB / T 28724-2012 "Determination of melting point of solid organic chemicals - Differential scanning calorimetry" to determine the melting point T of the sample. m ; The corrosion resistance of the sample is determined by referring to the standard QB / T 3801-1999 "Corrosion test method for rigid polyvinyl chloride pipes for chemical industry"; the flame retardant performance is determined by referring to the standard GB / T 2408-2021 "Horizontal and vertical methods for determination of combustion performance of plastics" to determine the combustion level of the sample. The specific test results are shown in the table below:

[0087]

[0088] Data Analysis:

[0089] By comparing and analyzing the data in the above table, the high-strength composite resin for wind tube processing prepared by the present invention has a bending strength of 354MPa, a breaking deflection of 8.6mm, and a notched impact toughness of 5.5kJ / m 2 The melting point (softening temperature) reaches 348°C and the corrosion degree reaches 0.15g / m 2, all the test data are better than those of the comparative example, indicating that the present invention prepares a composite resin material with good compatibility and high cross-linking degree by synthesizing a resin reinforcing agent containing a large number of siloxane bonds, olefin double bonds and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide-modified polysiloxane long chains and a matrix resin containing a large number of benzene rings and hydroxyl modifications, and then using reinforcing fibers, the resin reinforcing agent and the matrix resin. This not only effectively improves the bending performance and impact resistance of the composite resin, but also improves the high temperature resistance, corrosion resistance and combustion grade of the composite resin.

[0090] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

[0091] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0092] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for processing a high-strength composite resin for air duct processing, characterized in that: The following steps are involved: S1, adding modified polysiloxane and acetone into a three-necked flask protected by nitrogen and stirring, slowly dropping 3-isocyanate propylene into the three-necked flask, after the dropping is completed, raising the temperature of the three-necked flask to 40-50° C., keeping the temperature for reaction for 2-3 hours, and post-treating to obtain intermediate I, wherein the amount ratio of modified polysiloxane, acetone and 3-isocyanate propylene is 6g:18mL:1g; S2, adding intermediate I, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, n-propanol and catalyst into a three-necked flask and stirring, raising the temperature of the three-necked flask to 75-85° C., keeping the temperature for reaction for 8-10 hours, and post-treating to obtain intermediate II, wherein the amount ratio of intermediate I, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, n-propanol and catalyst is 10g:0.6g:30mL:0.1g; S3, adding intermediate II and acetone into a three-necked flask protected by nitrogen and stirring, slowly adding isocyanate propyl triethoxysilane into the three-necked flask, raising the temperature of the three-necked flask to 45-50°C, keeping the temperature for reaction for 6-8h, and post-treating to obtain a resin reinforcing agent, wherein the amount ratio of intermediate II, acetone and isocyanate propyl triethoxysilane is 3g:10mL:1g; S4, adding the base resin and acetone into a beaker, heating and stirring until the system is dissolved, adding reinforcing fiber and resin reinforcing agent into the beaker, stirring evenly, vacuum degassing, adding it into a mold, cooling and molding, demolding, and obtaining a composite resin; The modified polysiloxane is processed by the following steps: A1. Add methyldiethoxysilane, dimethyldiethoxysilane and anhydrous ethanol into a three-necked flask and stir. Add 10 wt % sodium hydroxide solution into the three-necked flask. Raise the temperature of the three-necked flask to a micro-reflux state. Keep the temperature for 6-8 hours and perform post-treatment to obtain polysiloxane. A2. Add polysiloxane, propylene alcohol and catalyst into a three-necked flask and stir. Raise the temperature of the three-necked flask to 80-90° C. and keep the temperature to react for 4-6 hours. Post-treat to obtain modified polysiloxane.

2. A method for processing a high-strength composite resin for processing a wind tube according to claim 1, characterized in that: In step S1, the post-processing operation includes: after the reaction is completed, the temperature of the three-necked flask is kept at 40-50° C., and the solvent is evaporated under reduced pressure to obtain intermediate I; in step S2, the catalyst is azobisisobutyronitrile, and the post-processing operation includes: after the reaction is completed, the temperature of the three-necked flask is kept at 75-85° C., and the solvent is evaporated under reduced pressure to obtain intermediate II; in step S3, the post-processing operation includes: after the reaction is completed, the solvent is evaporated under reduced pressure to obtain a resin reinforcing agent.

3. The method for processing a high-strength composite resin for processing a wind tube according to claim 1, characterized in that: In step A1, the amount ratio of methyldiethoxysilane and dimethyldiethoxysilane is 5mol:3mol, the amount ratio of dimethyldiethoxysilane, anhydrous ethanol and 10wt% sodium hydroxide is 1g:5mL:2mL, and the post-treatment operation includes: after the reaction is completed, the temperature of the three-necked flask is reduced to room temperature, hydrochloric acid is added to the three-necked flask, the pH of the system is adjusted to 7, the temperature of the three-necked flask is increased to 70-80°C, the solvent is evaporated under reduced pressure, anhydrous ethanol is added to the three-necked flask, suction is filtered, and the filtrate is transferred to a rotary evaporator, and the water bath temperature is set to 55-65°C to evaporate ethanol under reduced pressure to obtain polysiloxane.

4. The method for processing a high-strength composite resin for processing a wind tube according to claim 1, characterized in that: In step A2, the weight ratio of polysiloxane, acryl alcohol and catalyst is 6:1:0.3, the catalyst is 10wt% chloroplatinic acid / isopropanol solution, and the post-treatment operation includes: after the reaction is completed, the temperature of the three-necked flask is increased to 90-100° C., and the reduced pressure distillation is performed until no liquid flows out to obtain modified polysiloxane.

5. The method for processing a high-strength composite resin for processing a wind tube according to claim 1, characterized in that: The preparation method of the matrix resin is as follows: 4,4'-di(methoxymethyl)diphenyl ether, phenol and a catalyst are added into a three-necked flask and stirred, the temperature of the three-necked flask is increased to 120-130°C, the pressure is reduced to -0.1MPa, and the reaction is carried out by heat preservation for 2-3h, the temperature of the three-necked flask is reduced to 80-90°C, polyformaldehyde is added into the three-necked flask, the pressure of the three-necked flask is reduced to -0.1MPa, and the reaction is carried out by heat preservation for 2-3h to obtain the matrix resin.

6. A method for processing a high-strength composite resin for processing a wind tube according to claim 5, characterized in that: The dosage ratio of the 4,4'-bis(methoxymethyl)diphenyl ether to phenol is 1 mol:2 mol, and the weight ratio of the phenol, catalyst and paraformaldehyde is 10: 0.1:11, the catalyst is sodium hydroxide.

7. The method for processing a high-strength composite resin for processing a wind tube according to claim 1, characterized in that: In step S4, the weight ratio of the matrix resin, acetone, reinforcing fiber and resin reinforcing agent is 10:15:5:7, and the reinforcing fiber is one or more of glass fiber, polyester fiber, polypropylene fiber, carbon fiber and aramid fiber.