Fireproof and heat-resistant polyamide composition and preparation method and application thereof
By using fire-resistant and heat-resistant polyamide materials composed of aliphatic polyamides, halogen-free flame retardants, glass fibers and epoxy resins in lithium battery compositions, the lack of fire resistance and heat dissipation in high-temperature flames is solved. The problem has achieved efficient flame barrier and structural strength improvement in new energy vehicle lithium batteries.
Patent Information
- Application Number
- CN202311746970.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-12-19
Smart Images

Figure CN117683345B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer materials, and in particular relates to a fireproof and heat-resistant polyamide composition and a preparation method and application thereof. Background Art
[0002] In recent years, the new energy vehicle industry has entered a stage of vigorous development. New energy vehicle companies have used lithium batteries on a large scale in power batteries. Lithium batteries are high-energy bodies, and their charging and discharging is a violent heating process. Thermal runaway is one of the most common safety hazards of lithium batteries. Internal short circuits, overcharging, overdischarging and high temperatures are the main causes of thermal runaway. Thermal runaway of electric vehicles can cause battery combustion and surrounding parts to catch fire, and even explosions in severe cases.
[0003] GB 38031-2020 Safety Requirements for Power Batteries for Electric Vehicles requires that after thermal runaway of electric vehicle battery cells, the battery system will not catch fire or explode within 5 minutes, which helps ensure that drivers have enough time to evacuate and extinguish fires. This requires that the battery pack housing has excellent flame retardant properties and can effectively delay the spread of flames in the event of an electric vehicle fire. The improvement of regulations and safety standards will accelerate the technical improvement of related products, further enhance product quality and ensure product safety through technological innovation.
[0004] Aluminum alloy is currently the main material for battery casings. Aluminum alloy has advantages such as high strength and excellent heat dissipation, but its disadvantages cannot be ignored. Aluminum alloy casings have a large specific gravity and a complex manufacturing process. In addition, aluminum is highly chemically reactive with water at high temperatures, so it is difficult to extinguish a fire with water. Improper handling can lead to greater disasters. Traditional flame-retardant polymers usually use bromine, inorganic phosphorus or organic phosphorus to provide flame suppression, but this material can only support tens of seconds when exposed to flames and cannot meet the needs of power battery thermal runaway application scenarios. Moreover, the thermal conductivity of traditional flame-retardant polymer materials is relatively low, and there is also a heat dissipation problem when used in battery casings. Poor heat dissipation will lead to loss of battery life.
[0005] As one of the most ideal materials for lightweight and efficient structural design, polyamide composite materials have the advantages of high specific strength, corrosion resistance, fatigue resistance, good dimensional stability and strong design, and are very suitable for replacing aluminum alloys for battery pack housings and covers. Flame-retardant modified polyamide compositions usually add sufficient flame retardants to the formula to achieve flame suppression performance, such as patent document CN110461929A discloses a phosphite flame-retardant polyamide, patent document CN103328572A discloses a red phosphorus flame-retardant polyamide, and patent document CN102089373A discloses a melamine urate flame-retardant polyamide. However, these traditional flame-retardant polyamide composite materials can only resist flame burning for tens of seconds, and the flame retardant performance needs to be further improved. Patent document CN113646162A discloses a flame-retardant heat-insulating material suitable for battery cells, which has a three-layer structure, with aromatic polyamide and mica paper as the outer layer, and the inner layer is inorganic short fiber felt or paper. This method can well block the flame, but the disadvantage is that the design freedom of the product is not high. Patent document CN106133043A discloses a polyamide-based composition with fillers from the group including aluminum oxide, boron nitride and aluminum silicate, which is used to manufacture products with higher fire protection requirements, especially preferably products with higher glow wire (GWFI) requirements. This polyamide composite material is capable of contacting a glow wire (GWFI) of 960°C / 30 seconds, but is still far from blocking the flame for more than 5 minutes. Patent document CN111892814A discloses a high-barrier, fire-resistant, halogen-free, flame-retardant reinforced nylon composite material. By introducing linear phenolic resin into the phosphite flame-retardant nylon system, the material forms a micro-cross-linked structure during extrusion and injection molding, which can improve the density and strength of the carbon layer formed by the material during the combustion process, and greatly improve the thermal insulation capacity. This method directly adds phenolic resin to thermoplastic polymerization, and the thermosetting efficiency needs to be improved.
[0006] The known molding compositions are still insufficient in effectively delaying the flame spread time and fail to provide a composition having sufficient structural strength in a high temperature environment. Summary of the invention
[0007] In view of the above-mentioned deficiencies in the prior art, the main purpose of the present invention is to provide a fire-proof and heat-resistant polyamide composition, which is a polyamide composite material that can replace aluminum alloy for heat dissipation, will not melt, drip or perforate even when burned by flame for at least 5 minutes, and still has a certain structural strength after high temperature and burning.
[0008] Another object of the present invention is to provide a method for preparing the fire-resistant and heat-resistant polyamide composition.
[0009] Another object of the present invention is to provide an application of the fire-resistant and heat-resistant polyamide composition in the preparation of a new energy vehicle lithium battery pack casing and a cover.
[0010] To achieve the above object, the present invention adopts the following technical solution:
[0011] The present invention provides a fire-proof and heat-resistant polyamide composition, comprising the following components:
[0012]
[0013] The sum of components (A) to (G) accounts for 100 wt % of the fire-resistant and heat-resistant polyamide composition.
[0014] Preferably, the aliphatic polyamide of component (A) is a semi-crystalline polymer having a melting temperature of 150-300° C. The melting temperature is characterized by differential scanning calorimetry (DSC) with a heating and cooling rate of 10° C. / min.
[0015] More preferably, the repeating units of the aliphatic polyamide are selected from one or more monomers of aliphatic dicarboxylic acids, aliphatic diamines having not less than four carbon atoms, and lactams; wherein:
[0016] The aliphatic dicarboxylic acid is selected from the group consisting of oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, octadecanedioic acid, eicosanedioic acid;
[0017] The aliphatic diamine having not less than four carbon atoms is selected from the group consisting of butanediamine, pentamethylenediamine, ethylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, tridecanediamine, tetradecanediamine, pentadecanediamine, hexadecanediamine, heptadecanediamine, octadecanediamine, nonadecanediamine, eicosanediamine, 2-methyl-1,8-octanediamine, 2,2,4-trimethylhexamethylenediamine, 2,4,4-trimethylhexamethylenediamine;
[0018] The lactam is selected from the group consisting of: ε-caprolactam, enantholactam, undecanolactam, dodecanolactam, α-pyrrolidone, and α-piperidone.
[0019] In some preferred embodiments, the aliphatic polyamide and monomer are selected from one or more of the following:
[0020] Aliphatic polyamide monomer PA 6 ε-Caprolactam PA 66 Hexamethylenediamine, adipic acid PA 610 Hexamethylenediamine, sebacic acid PA 612 Hexamethylenediamine, dodecanedioic acid PA 46 Butanediamine, adipic acid PA 56 Pentamethylenediamine, adipic acid PA 1010 Decanediamine, Sebacic acid PA 11 Undecanolactam PA 12 Dodecanolactam
[0021] In some preferred embodiments, the aliphatic polyamide is PA 66 and / or PA 6.
[0022] Preferably, component (B) is a halogen-free flame retardant, which is a dialkyl phosphinate represented by formula (I); or a mixture of a dialkyl phosphinate represented by formula (I) and a phosphite represented by formula (II); or a mixture of a dialkyl phosphinate represented by formula (I), melamine polyphosphate and zinc borate;
[0023]
[0024] In formula (I), R 1 , R 2 are the same or different and represent a linear or branched C1-C6 alkyl group;
[0025] M1 represents Mg, Ca, Al, Sb, Sn, Ge, Ti, Zn, Fe, Zr, Ce, Bi, Sr, Mn, Li, Na, K and / or a protonated nitrogen base; m represents an integer from 1 to 4; n represents an integer from 1 to 4;
[0026]
[0027] In formula (II), M2 represents Mg, Ca, Al, Sb, Sn, Ge, Ti, Zn, Fe, Zr, Ce, Bi, Sr, Mn, Li, Na, K; m represents an integer from 1 to 4.
[0028] The halogen-free flame retardants represented by formula (I) and (II) are described in patent CN103154110B and can be purchased commercially.
[0029] More preferably, when the halogen-free flame retardant is a mixture, the content of the dialkyl phosphinate represented by formula (I) is higher than 70%, preferably higher than 80%, and more preferably higher than 90%.
[0030] In some embodiments, the flame retardant is aluminum diethylphosphinate 3 (C4H 10 O2P).Al), or diethylphosphinate aluminum 3 (C4H 10 A mixture of Al and aluminum hypophosphite Al2(HPO3)3, or diethylphosphinate aluminum 3(C4H 10 O2P).Al, melamine polyphosphate and zinc borate. When the halogen-free flame retardant is a mixture, diethylphosphinate aluminum 3 (C4H 10 O2P).Al ratio is higher than 70%, preferably higher than 80%, more preferably higher than 90%.
[0031] Preferably, component (C) is glass fiber selected from round cross-section glass fiber and / or flat cross-section glass fiber.
[0032] The flat cross-section glass fiber refers to a glass fiber with a certain thickness-to-width ratio cross section, and the cross section can have a variety of shapes, including rectangular, elliptical and approximately elliptical, and the shape ratio (ratio of the short axis length to the long axis length) is in the range of 1:1.5 to 6, more preferably in the range of 1:2 to 5, and more preferably in the range of 1:3 to 4.
[0033] Preferably, component (D) is a ceramic mineral selected from at least 60 wt% of kyanite and 0 to 40 wt% of one or more of spherical alumina, titanium dioxide and boron nitride; wherein:
[0034] The kyanite is a triclinic aluminum silicate mineral with a chemical formula of A2SiO5 and a typical chemical composition of 63.3% Al2O3 and 36.7% SiO2. The term "triclinic system" is understood by ordinary technicians in the field to mean a crystal structure with neither a higher-order symmetry axis nor a secondary axis and a symmetry plane, and its three crystal axes are mutually oblique, the unit cell axis distance a≠b≠c, and the axis angle α≠β≠γ≠90°( Figure 2 ). Triclinic kyanite is an unstable phase at high temperature and has a low sintering temperature. When the heating temperature exceeds 1100°C, it decomposes into mullite and fused silica glass through the following reactions:
[0035] 3(Al2O3·SiO2)→3Al2O3·2SiO2+SiO2
[0036] This transformation helps to increase the load softening temperature and compressive strength, which can provide supporting strength for the product in the flame.
[0037] As a preferred component (E) is an epoxy resin, which means that the molecule contains two or more epoxy groups. In the compounds, the epoxy group can be located at the end, in the middle or in a ring structure of the molecular chain.
[0038] The epoxy resin is not particularly limited, and compounds having two or more glycidyl groups in one molecule can be cited. In addition, the epoxy resin selected can be appropriately used by condensing epichlorohydrin with polyphenols such as bisphenols or polyols under the action of an alkaline catalyst (usually sodium hydroxide).
[0039] In some embodiments, the epoxy resin is selected from one or more of bisphenol A epoxy resin, bisphenol F epoxy resin, and novolac epoxy resin.
[0040] The epoxy resin preferably has an epoxy equivalent weight (Eew) in the range of 100 to 600 g / eq. The Eew of the epoxy resin is the amount of resin containing one epoxy group (g / eq), that is, the average molecular weight of the epoxy resin divided by the number of epoxy groups contained in each molecule. The Eew of the epoxy resin affects the addition ratio of the curing agent.
[0041] The bisphenol A type epoxy resin is not particularly limited, and a wide range of epoxy resins that can be used for thermoplastic modification can be used. As a preferred example, DER produced by Olin Corporation of the United States TM 671, eew is 475~550g / eq.
[0042] The bisphenol F type epoxy resin is not particularly limited, and a wide range of epoxy resins that can be used for thermoplastic modification can be used. As a preferred example, DER produced by Olin Corporation of the United States TM 354, eew is 167~174g / eq.
[0043] The novolac epoxy resin is not particularly limited, and a wide range of epoxy resins that can be used for thermoplastic modification can be used. As a preferred example, for example, epoxy resins produced by DIC Corporation of Japan N-775, eew is 180~200g / eq.
[0044] Component (F) is a latent curing agent, the properties of which are well known to technicians. After being added to the epoxy resin, it has good storage stability at room temperature and can quickly react chemically with the epoxy resin at high temperatures to eventually form a tough network-like three-dimensional polymer.
[0045] Preferably, the latent curing agent is dicyandiamide (DICY) represented by formula (III), or one or a mixture of two of modified DICY compounds having formula (III) as a basic skeleton:
[0046]
[0047] Among them, the melting point of DICY is 208-211°C. In addition to 4 active hydrogen atoms in its molecular structure, it also contains cyano (-CN), which can also participate in the curing reaction as a functional group. DICY is a widely used heat-curing latent curing agent. Once heated to near the melting point, DICY begins to dissolve and begins to react with the epoxy resin. The curing reaction temperature of dicyandiamide is generally 160-180°C, and the curing reaction time is 20-60 minutes. The cured product of dicyandiamide has good mechanical properties and heat resistance.
[0048] DICY is commercially available, and a preferred example is DICY50 produced by Mitsubishi Chemical Corporation of Japan.
[0049] Modified DICY refers to a compound having DICY as a basic skeleton and exhibiting a curing-accelerating effect, and includes, in addition to the DICY structure itself, a compound having a structure in which a part of the hydrogen atoms of the amino group of DICY are replaced. Modified DICY derivatives are commercially available, and as a preferred specific example, AH-154 produced by Ajinomoto Co., Ltd. of Japan is one example.
[0050] Preferably, the amount of DICY and modified DICY added should be appropriately set in consideration of the epoxy equivalent of the epoxy resin. Preferably, the ratio of the active hydrogen equivalent of the latent curing agent to the epoxy equivalent of the epoxy resin is 0.05 to 0.25, more preferably 0.1 to 0.2.
[0051] Active hydrogen equivalent refers to the number of active hydrogen atoms contained in a molecule, which can be calculated according to formula (IV). Active hydrogen atoms refer to hydrogen atoms with higher electron affinity in a molecule. In chemical reactions, active hydrogen atoms have strong electrophilicity and are easy to react chemically with other atoms or molecules.
[0052]
[0053] The molecular weight of dicyandiamide is 84, and its molecular structure contains 4 active hydrogen atoms, with an active hydrogen equivalent of 21.
[0054] Preferably, component (G) is other auxiliary agents, selected from one or a mixture of two or more of a colorant, a release agent, a heat stabilizer, a flow improver and a crystallization accelerator.
[0055] The present invention also provides a method for preparing the fireproof and heat-resistant polyamide composition, which is obtained by heating, melting, blending and extruding through a single-screw or twin-screw extruder.
[0056] Preferably, the length-to-diameter ratio (L / D) of the single-screw or twin-screw extruder is 32-52, preferably L / D is 40-44.
[0057] Preferably, the processing temperature is set to 150-300° C., and the screw speed is set to 200-500 rpm.
[0058] Preferably, the process of heating, melting, blending and extruding comprises:
[0059] Adding sequence: a side feeding port is set at the rear section of the single-screw or twin-screw extruder for heating and melting, and component (B) flame retardant, component (C) glass fiber and component (G) latent curing agent are added. Other material components are metered and added from the main feeding port of the extruder after premixing;
[0060] Exhaust: 1 to 2 barrel holes in front of the extruder feeding port are used for normal pressure exhaust, and the second to last barrel hole in the die head is used for pressurized exhaust, with a pressure range of 30 to 70 cm-Hg;
[0061] The melt from the twin-screw extruder is extruded through a die, cooled in a water tank, and cut into granules by a pelletizer. The collected granules are dried to a moisture content of less than 0.1% and then packaged.
[0062] The present invention also provides the use of the fireproof and heat-resistant polyamide composition in preparing a housing and a cover of a lithium battery pack for a new energy vehicle.
[0063] Compared with the prior art, the present invention has the following beneficial effects:
[0064] The fireproof and heat-resistant polyamide composition of the present invention is filled with a thermally conductive filler mainly composed of triclinic kyanite, and the thermal conductivity is improved by several to dozens of times compared with traditional polymer materials, which can improve heat dissipation and help reduce thermal runaway of the battery. In addition, the sintering temperature of triclinic minerals is low, which can provide supporting strength for the product in the flame. Secondly, a latent thermosetting system is introduced into the thermoplastic polymer, which not only retains the characteristics of plasticity, but also ensures that the components maintain dimensional stability under battery operating conditions, and further enhances the ability of the combination to resist flames. According to tests, the fireproof and heat-resistant polyamide composition of the present invention can withstand direct flame exposure of 1000°C for more than 15 minutes, and can provide passengers with enough time to leave the vehicle when thermal runaway occurs. BRIEF DESCRIPTION OF THE DRAWINGS
[0065] Figure 1 Schematic diagram of flame exposure test of the specimen in the embodiment.
[0066] Figure 2 Schematic diagram of the crystal structure model of triclinic kyanite.
[0067] Figure 3 This is a photograph of the test piece of Comparative Example 1 after being exposed to flame for 1 minute.
[0068] Figure 4 This is a photograph of the test piece of Example 1 after being exposed to flame for 15 minutes.
[0069] Figure 5 The mechanical properties test results of the test pieces of Example 1 and Comparative Example 1 after flame exposure. DETAILED DESCRIPTION
[0070] The present invention is further described by the following examples. It should be understood that the following examples are for illustrative purposes only and are not intended to limit the present invention.
[0071] The following materials were used in the Examples and Comparative Examples:
[0072] PA 66: Polyamide 66 produced by Ningxia Ruitai Company.
[0073] PA 6: Polyamide 6 produced by Luxi Chemical Company.
[0074] PA610: Polyamide 610 produced by Guangyin Company.
[0075] PA612: Polyamide 612 produced by Guangyin Company.
[0076] PA46: Polyamide 46 produced by DSM.
[0077] PA 56: Polyamide 56 produced by Cathay.
[0078] PA 1010: Polyamide 1010 produced by Guangyin Company.
[0079] PA11: Polyamide 11 produced by Emmans.
[0080] PA 12: Polyamide 12 produced by Wanhua.
[0081] MIX-PA: refers to a mixture of PA 610: PA 612: PA 46: PA 56: PA 1010: PA 11: PA 12 in the ratio of 1:1:1:1:1:1:1, obtained by Jinlun Company.
[0082] GF-1: Round cross-section glass fiber 995-10P produced by Shandong Fiberglass Company, with a single fiber diameter of 10μm.
[0083] GF-2: Flat glass fiber ECS301 HP-3-M4 produced by Chongqing International Composite Materials Co., Ltd., with a profile ratio of 1:4.
[0084] FR-1: Aluminum diethylphosphinate produced by Clariant, brand OP1230.
[0085] FR-2: A mixture of aluminum diethylphosphinate, melamine polyphosphate and zinc borate produced by Clariant, with the proportion of aluminum diethylphosphinate being about 70% to 80%.
[0086] FR-3: A mixture of aluminum diethylphosphinate and aluminum hypophosphite produced by Clariant, with the proportion of aluminum diethylphosphinate being about 90%.
[0087] MIX-FR means The mixture was obtained by mixing by Jinlun Company in the ratio of 1:1:1.
[0088] Kyanite: Kyanite from American Kyanite Mining, 100 mesh.
[0089] AL2O3: Spherical alumina produced by Yishitong Company.
[0090] TIO2: Rutile titanium dioxide produced by Coster, Australia, brand RCL-69.
[0091] BN: Boron nitride produced by 3M Company in the United States, brand CFA50M.
[0092] MIX-MD: refers to a mixture of spherical alumina: titanium dioxide RCL-69: boron nitride CFA50M in a ratio of 1:1:1, obtained by Jinlun Company.
[0093] Epoxy-1: Bisphenol A epoxy resin DER produced by Olin Corporation in the United States TM 671, epoxy equivalent 475-550g / eq.
[0094] Epoxy-2: Bisphenol F epoxy resin DER produced by Olin Corporation in the United States TM 354, epoxy equivalent 167-174g / eq.
[0095] Epoxy-3 is a phenolic varnish epoxy resin produced by DIC of Japan. N-775, epoxy equivalent 180-200g / eq.
[0096] DICY-1: DICY50 produced by Mitsubishi Chemical Corporation of Japan, with an active hydrogen equivalent of 21g / eq.
[0097] DICY-2: A modified dicyandiamide compound AH-154 produced by Ajinomoto Co., Ltd. of Japan, with an active hydrogen equivalent of 17g / eq.
[0098] 1098: Antioxidant 1098 produced by BASF, with the chemical name N,N'-bis-(3-(35-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine.
[0099] Black MB: PA6 carrier / 40% carbon black masterbatch SC8715 produced by Ningbo Masterbatch Factory.
[0100] CaSt2: refers to calcium stearate SAK-CS-P produced by Singapore Samyuk Company.
[0101] Preparation method
[0102] The components were weighed as shown in Table 1 and then added to a twin-screw extruder for melt processing.
[0103] Extruder screw nominal diameter: 35mm.
[0104] Extruder screw aspect ratio: 40.
[0105] Processing temperature range: 150~300℃.
[0106] Main engine speed range: 300rpm.
[0107] Feeding sequence: a side feeding port is set at the rear section of the extruder for heating and melting, and component (B) flame retardant, component (C) reinforcing agent and component (G) latent curing agent are added. Other material components are metered and added from the main feeding port of the extruder after premixing.
[0108] Exhaust: 1 to 2 barrel openings in front of the extruder feeding port are used for normal pressure exhaust, and the second to last barrel opening in the die head is used for pressurized exhaust. The pressure range is 30 to 70 cm-Hg.
[0109] The melt from the twin-screw extruder is extruded through a die, cooled in a water tank, and cut into granules by a pelletizer. The collected granules are dried to a moisture content of less than 0.1% and then packaged.
[0110] Specimen molding and conditioning
[0111] The specimen molding and conditioning are carried out according to the method specified in ISO 16396-2, with the molding melt temperature of 250-300°C and the mold temperature of 80-100°C. For the mechanical properties test, the specimen is placed in an environment of 23°C for conditioning for more than 16 hours, and the moisture content of the specimen is ensured to be less than 0.2%. For the flammability test, the specimen is subjected to two pre-conditioning conditions: 23°C / 50%RH / 48 hours and 70°C / 168 hours.
[0112] Thermal conductivity test
[0113] Thermal conductivity refers to the amount of heat transferred through an area of 1 square meter in 1 second under stable heat transfer conditions when the temperature difference between the two surfaces of a 1m thick material is 1 degree (K, ℃). It is represented by the symbol λ and its unit is W / (mK).
[0114] The thermal conductivity calculation formula is λ=ρ×a×Cp, where:
[0115] ρ-Material density, obtained by immersion test;
[0116] a- thermal diffusion coefficient, measured by laser flash method;
[0117] Cp-specific heat capacity, measured by DSC method.
[0118] Flammability test
[0119] The V-level vertical combustion test was carried out according to the method specified in UL94. The test piece size was 125mm×13.0mm×1.5mm, the methane blowtorch flame height was 20mm, the inner flame height was 10mm, and the test instrument was the ATLAS HVUL2 combustion box.
[0120] Flame exposure test
[0121] The flame height of the methane blowtorch is 125 mm, the inner flame height is 40 mm, the flame temperature is 1100°C, the blowtorch angle is 20±5°, and the test instrument is the ATLAS HVUL2 combustion box.
[0122] Two sizes of test pieces are provided for testing: the test piece used to evaluate appearance is 80mm×80mm×2mm in size, and the test piece used to evaluate mechanical properties is 80mm×10mm×4.0mm in size.
[0123] like Figure 1 As shown, during the test, the test piece is fixed horizontally and the height is adjusted so that the inner flame of the flame contacts the center of the sample. If the test piece is cracked or perforated after contacting the flame, the test is stopped and the time is recorded.
[0124] Mechanical properties test
[0125] The bending performance was tested according to the method specified in ISO178. The test piece size was 80 mm × 10 mm × 4 mm. The pressing speed was 2 mm / min. The testing instrument was a ZWICK Z010 universal testing machine.
[0126] High temperature exposure test
[0127] The test piece has a size of 80 mm × 10 mm × 4 mm. The test piece is placed in an oven (enclosed environment) and different ambient temperatures are set. After the temperature is raised to the set temperature, the temperature is kept constant for 10 minutes, and then the test piece is taken out for appearance evaluation. The test instrument is a Memmert UF110 oven.
[0128] Examples and Comparative Examples
[0129] Table 1 and Table 2, Figure 3-5 The composition performance of each example is listed.
[0130] Compared with Comparative Example 1 and Comparative Example 4: After 20% kyanite was added to Comparative Example 4, the flame exposure performance was significantly improved compared with Comparative Example 1, and the composition could withstand flame exposure for 15 minutes while maintaining structural integrity, indicating that the fire resistance of the composition was improved after the addition of kyanite, but both solutions failed in the high temperature exposure test after exceeding the melting point of the substrate PA66 (260°C).
[0131] Compared with Comparative Example 1 and Comparative Example 5: After adding 5% epoxy resin and 0.2% curing agent to Comparative Example 5, the flame exposure resistance and high temperature exposure performance are improved. Comparative Example 5 can still maintain structural integrity in an ambient temperature exceeding the melting point of the substrate PA66 (260°C), indicating that the composition is cross-linked and cured due to the addition of epoxy resin and curing agent, thereby improving the fire resistance and high temperature exposure performance of the composition.
[0132] Comparison of Example 5, Example 1 and Example 3: The proportions of kyanite in the three compositions are 0%, 20% and 50% respectively. It can be observed that as the proportion of kyanite increases, the flame resistance of the composition is further improved. However, too high a proportion of kyanite will affect the processing performance, so it is necessary to control the proportion of kyanite to a reasonable proportion.
[0133] Compared with Comparative Examples 7, 8 and 9: the proportions of epoxy resin in the three combinations are 3%, 5% and 10%, respectively, but no improvement was observed in the flame exposure and high temperature exposure performance of the compositions, indicating that the epoxy resin cannot be cured to form a tough network three-dimensional polymer without the participation of a curing agent.
[0134] In Examples 5 to 10, epoxy resins with different proportions and different epoxy equivalents are selected, and the addition ratio of the curing agent is calculated according to the formula: Curing agent ratio (%) = hydrogen equivalent / epoxy equivalent × 100. The test shows that after adding a reasonable proportion of the curing agent, the epoxy resin in the composition can be cured smoothly, thereby improving the fireproof and heat resistance of the composition.
[0135] Table 1
[0136]
[0137]
[0138] Note: Appearance evaluation: O = structural integrity; △ = obvious structural deformation; × = structural failure (burn through or melt).
[0139] Table 2
[0140]
[0141]
[0142] Note: Appearance evaluation: O = structural integrity; △ = obvious structural deformation; × = structural failure (burn through or melt).
[0143] The above is only a preferred embodiment of the present invention, but the present invention should not be limited to the contents disclosed in the embodiment. Therefore, any equivalent or modification completed without departing from the spirit disclosed in the present invention shall fall within the scope of protection of the present invention.
Claims
1. A fireproof and heat-resistant polyamide composition, characterized in that: The fireproof and heat-resistant polyamide composition comprises the following components: wherein the sum of the components accounts for 100 wt% of the fire-resistant and heat-resistant polyamide composition; The aliphatic polyamide is a semi-crystalline polymer with a melting temperature of 150 to 300°C; The repeating units of the aliphatic polyamide are selected from one or more monomers of aliphatic dicarboxylic acid, aliphatic diamine having not less than four carbon atoms, and lactam, wherein: The aliphatic dicarboxylic acid is selected from the group consisting of oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, octadecanedioic acid, and eicosanedioic acid; The aliphatic diamine having not less than four carbon atoms is selected from the group consisting of butanediamine, pentamethylenediamine, ethylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, tridecanediamine, tetradecanediamine, pentadecanediamine, hexadecanediamine, heptadecanediamine, octadecanediamine, nonadecanediamine, eicosanediamine, 2-methyl-1,8-octanediamine, 2,2,4-trimethylhexamethylenediamine, and 2,4,4-trimethylhexamethylenediamine; The lactam is selected from the group consisting of: ε-caprolactam, enantholactam, undecanolactam, dodecanolactam, α-pyrrolidone, α-piperidone; The flame retardant is a halogen-free flame retardant selected from a dialkyl phosphinate represented by formula (I); or a mixture of a dialkyl phosphinate represented by formula (I) and a phosphite represented by formula (II); or a mixture of a dialkyl phosphinate represented by formula (I), melamine polyphosphate and zinc borate; In formula (I), R 1 、R 2 are the same or different and represent a linear or branched C1-C6 alkyl group; M1 represents Mg, Ca, Al, Sb, Sn, Ge, Ti, Zn, Fe, Zr, Ce, Bi, Sr, Mn, Li, Na, K and / or a protonated nitrogen base; m represents an integer from 1 to 4; n represents an integer from 1 to 4; In formula (II), M2 represents Mg, Ca, Al, Sb, Sn, Ge, Ti, Zn, Fe, Zr, Ce, Bi, Sr, Mn, Li, Na, or K; m represents an integer from 1 to 4; When the halogen-free flame retardant is a mixture, the content of the dialkyl phosphinate represented by formula (I) is higher than 70%; The ceramic mineral is selected from a mixture of at least 60 wt% of kyanite and 0 to 40 wt% of one or more of spherical alumina, titanium dioxide, and boron nitride, wherein the kyanite is a triclinic aluminum silicate mineral with a chemical formula of A2SiO5 and a chemical composition of 63.3% Al2O3 and 36.7% SiO2; The latent curing agent is dicyandiamide represented by formula (III), or one or a mixture of two modified dicyandiamide compounds having formula (III) as a basic skeleton:
2. The fireproof and heat-resistant polyamide composition according to claim 1, characterized in that: The melting temperature was characterized by differential scanning calorimetry, with a heating and cooling rate of 10° C. / min.
3. The fireproof and heat-resistant polyamide composition according to claim 1, characterized in that: The aliphatic polyamide and monomer are selected from one or more of the following:
4. The fireproof and heat-resistant polyamide composition according to any one of claims 1 to 3, characterized in that The aliphatic polyamide is PA66 and / or PA6.
5. The fireproof and heat-resistant polyamide composition according to claim 1, characterized in that: The flame retardant is aluminum diethylphosphinate, or a mixture of aluminum diethylphosphinate and aluminum hypophosphite, or a mixture of aluminum diethylphosphinate, melamine polyphosphate and zinc borate; when the flame retardant is a mixture, the content of aluminum diethylphosphinate is higher than 70%.
6. The fireproof and heat-resistant polyamide composition according to claim 1, characterized in that: The glass fiber is selected from circular cross-section glass fiber and / or flat cross-section glass fiber, the cross-section of the flat cross-section glass fiber is selected from one or more of rectangular, elliptical and nearly elliptical shapes, and the shape ratio is 1:1.5 to 6; the other additives are selected from one or a mixture of two or more of a colorant, a release agent, a heat stabilizer, a flow improver and a crystallization promoter.
7. The fireproof and heat-resistant polyamide composition according to claim 1, characterized in that: The epoxy resin is selected from one or more of bisphenol A epoxy resin, bisphenol F epoxy resin, and novolac epoxy resin, and has an epoxy equivalent of 100 to 600 g / eq.
8. The fireproof and heat-resistant polyamide composition according to claim 1, characterized in that: The ratio of the active hydrogen equivalent of the latent curing agent to the epoxy equivalent of the epoxy resin is 0.05 to 0.25:
1.
9. The method for preparing the fireproof and heat-resistant polyamide composition according to any one of claims 1 to 8, characterized in that: The mixture is obtained by heating, melting and blending in a single-screw or twin-screw extruder; wherein: The single-screw or twin-screw extruder has an aspect ratio L / D of 32 to 52; The processing temperature is 150-300°C, and the screw speed is 200-500rpm.
10. The method for preparing the fireproof and heat-resistant polyamide composition according to claim 9, characterized in that: The process of heating, melting and blending extrusion comprises: Feeding order: set a side feeding port at the rear section of the single-screw or twin-screw extruder for heating and melting, add flame retardant and glass fiber, and add other material components through the main feeding port of the extruder after premixing; Exhaust: 1 to 2 barrel openings in front of the extruder feed port are used for normal pressure exhaust, and the second-to-last barrel opening in the die head is used for pressurized exhaust. The pressure range is 30 to 70 cm-Hg. The melt from the twin-screw extruder is extruded through a die, cooled in a water tank, and then cut into granules by a pelletizer. The collected granules are dried to a moisture content of less than 0.1% and then packaged.
11. Use of the fireproof and heat-resistant polyamide composition according to any one of claims 1 to 8 in preparing housings and covers of lithium battery packs for new energy vehicles.