A method for controlling the length of the tail billet when the casting is stopped

By increasing the upper steel temperature, detecting the length of the tail billet in real time, adjusting the blocking sequence, cooling and then pulling down, and controlling the specific water volume of the tail billet, the problem of tail billet length control during the continuous casting process was solved, and precise control of the tail billet length was achieved, improving It improves the casting yield and production efficiency, and reduces the cost and labor intensity.

CN117718455BActive Publication Date: 2024-10-29SHANDONG IRON & STEEL GRP YONGFENG LINGANG CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410126012.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-30
Publication Date
2024-10-29
Estimated Expiration
2044-01-30

AI Technical Summary

Technical Problem

At the end of the continuous casting process, the drop in molten steel level in the tundish and the change in casting speed lead to the involvement of vortex slag and molding slag, reducing the cleanliness and quality of the tail billet. The existing treatment methods lead to reduced product quality, energy waste and Increased costs.

Method used

By increasing the steel loading temperature of the stopped pouring furnace, the length of the tail billet is detected in real time and the flow blocking sequence is adjusted. After the flow is blocked, it is cooled and then pulled down to control the specific water volume of the tail billet. It is automatically cut after the tail billet is pulled out to achieve precise control of the length of the tail billet. .

Benefits of technology

It effectively controls the length of the tail billet to less than 1.5m, improves the casting yield, saves manual operation time and costs, improves the quality and production efficiency of the tail billet, and reduces the recycling cost.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the technical field of steel smelting, and in particular, relates to a method for controlling the length of the tail billet when the casting is stopped. The method comprises the following steps: (1) increasing the upper steel temperature of the stopping furnace; (2) blocking the flow according to the actual length of the tail billet; (3) controlling the blocking sequence; (4) cooling the tail billet after blocking the flow and then pulling it down; (5) controlling the water content of the tail billet; (6) after the tail billet is discharged, the fire cutting machine automatically cuts it according to the normal fixed length. The present invention can control the length of the tail billet of a single flow to be below 1.5m, thereby improving the yield of the casting billet. According to calculation, compared with the tail billet length of 3-4m in the prior art, the waste of the casting billet is reduced by 0.07kg / t, and the cost can be saved by more than 300,000 yuan per year.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of steel smelting, and in particular relates to a method for controlling the length of the tail billet when casting is stopped. Background Art

[0002] At the end of the continuous casting process, the continuous drop in the molten steel level in the tundish and the drastic change in the casting speed easily cause the vortex slag and protective slag to be drawn in, thereby reducing the cleanliness and quality of the tail billet. At present, various steel mills usually adopt the strategy of downgrading or scrapping the tail billet, but this method often results in "missed judgment" or "wrong judgment", resulting in a decrease in product quality and billet yield, energy waste and increased steel costs. The current treatment method for the tail billet after the billet casting is stopped has the following problems:

[0003] 1. After stopping pouring, the flow is blocked in turn according to the remaining molten steel in the tundish. In order to ensure the quality of the tail of the ingot, the average length of a single flow of the tail ingot is controlled at 3-4m. Each time the pouring is stopped for 8 flows, about 5t is wasted.

[0004] 2. When the casting of the tail billet is stopped and the single stream is 3-4m, it cannot enter the large roller table together with the last billet. It is necessary to direct the crane to use chains to lift it to the waste billet bucket one by one, which increases the labor intensity of the personnel.

[0005] 3. It takes about 25 minutes for two people to process the tail billet, which affects the efficiency of other operations during the shutdown.

[0006] 4. The tail billet hoisted into the waste billet bucket is too long and needs to be manually cut again to less than 2m, which increases the labor intensity of the operator. Summary of the invention

[0007] The object of the present invention is to provide a method for controlling the length of the tail billet when casting is stopped, so as to solve the problems existing in the prior art.

[0008] The technical solution adopted by the present invention to solve the technical problem is: a method for controlling the length of the tail billet when the casting is stopped, comprising the following steps:

[0009] (1) Increase the steel supply temperature of the furnace that stops pouring;

[0010] (2) Block the flow according to the actual length of the tail billet;

[0011] (3) Control the flow blocking sequence;

[0012] (4) Cool down first and then pull down after blocking the flow;

[0013] (5) Control the tail water volume;

[0014] (6) After the tail is out, the flame cutting machine automatically cuts according to the normal fixed length.

[0015] Furthermore, in step (1), the upper steel temperature of the stopped pouring furnace is increased from 1548°C to 1553°C.

[0016] Furthermore, in step (2), the flow is blocked according to the actual length of the tail billet. A length measuring instrument is installed in the operation box of each flow to detect the position and length of the tail billet in real time, and the flow is blocked according to the actual length of the tail billet.

[0017] Furthermore, in step (3), the blocking sequence of the flow is controlled as follows: for the last furnace before the tundish stops casting, when the weighing shows that there are 25 tons of molten steel in the tundish, the 1st and 8th streams on both sides are blocked first, and the remaining 6 streams continue to cast the remaining part, and the length measuring instrument is observed, and the flow is blocked in turn according to the actual length of the tail billet.

[0018] Furthermore, the total capacity of the middle package is 60t.

[0019] Furthermore, in step (4), after the flow is blocked, the casting is first cooled and then pulled down. When the flow is blocked, the casting is not pulled down directly, but the casting is allowed to stay in the crystallizer for 10 seconds to cool and then pulled down.

[0020] Furthermore, in step (5), the water content of the tail is controlled to be 1.2 L / kg, and the casting is designed to automatically run at a pulling speed of 2.5 m / min. After 2 minutes, the water content is adjusted to 1.0 L / kg, and the casting is automatically discharged at a speed of 2.0 m / min.

[0021] The present invention has the following beneficial effects:

[0022] 1. The present invention can control the length of the tail billet of a single stream to less than 1.5m, thereby improving the yield of the billet. According to calculations, compared with the tail billet length of 3-4m in the prior art, the waste of the billet is reduced by 0.07kg / t, and the cost can be saved by more than 300,000 yuan per year.

[0023] 2. Since the length of the tail billet is controlled below 1.5m, the lifting and cutting steps are omitted. The tail billet of 1.5m in length can enter the large roller along with the last complete billet, without the need to lift it stream by stream, thereby reducing labor, saving 25 minutes of tail billet lifting processing time, improving efficiency and reducing labor intensity.

[0024] 3. The tail billet put into the waste billet bucket is 1.5m long, which is suitable and does not need to be cut again, which further saves time, improves efficiency, saves cutting costs, and increases the reserved time for other operations.

[0025] 4. By cooling the product before pulling it down after blocking the flow and controlling the water content of the tail product, the quality of the tail product is improved and the cost of recycling the tail product is reduced. DETAILED DESCRIPTION

[0026] Taking 8-machine 8-stream continuous casting equipment as an example, a method for controlling the length of the tail billet after stopping casting of the billet comprises the following steps:

[0027] (1) Increase the steel supply temperature of the furnace that stops pouring;

[0028] (2) Block the flow according to the actual length of the tail billet;

[0029] (3) Control the flow blocking sequence;

[0030] (4) Cool down first and then pull down after blocking the flow;

[0031] (5) Control the tail water volume;

[0032] (6) After the tail is out, the flame cutting machine automatically cuts according to the normal fixed length.

[0033] In step (1), the upper steel temperature of the stopped pouring furnace is increased from 1548° C. to 1553° C. The upper steel temperature of the stopped pouring furnace is increased by 5° C. compared with the previous normal casting temperature.

[0034] When the last furnace is stopped, the casting speed needs to be slowed down, so the temperature drops quickly, resulting in a long tail billet, which is difficult to control at a reasonable length. According to actual machine experiments, the higher the upper steel temperature, the shorter the tail billet length, and the higher the power consumption. According to calculations, for every 1°C increase in the upper steel temperature, the power consumption increases by 80 degrees.

[0035] Therefore, when shortening the length of the tail billet by increasing the upper steel temperature, the electricity consumption cost also needs to be considered. When the upper steel temperature is increased by 5°C, the average length of the tail billet is less than 1.5m. Under this tail billet length, there is no need to manually lift the tail billet of each flow, nor is there any need to cut it again. The tail billet only needs to be put into the large roller together with the last billet, so the lifting and cutting steps are omitted, thereby reducing labor, saving time, and improving efficiency. At the same time, the yield of the billet is increased. Although the electricity consumption increases, the benefits brought by this are higher than the increase in electricity consumption costs.

[0036] In step (2), the flow is blocked according to the actual length of the tail billet. A length measuring instrument is installed in the operation box of each flow to detect the position and length of the tail billet in real time, and the flow is blocked according to the actual length of the tail billet.

[0037] In view of the current situation that the tail billet length control is not accurate during flow blockage, a length measuring instrument is used to detect the tail billet position and length in real time, so as to more accurately control the tail billet length and ensure that the tail billet length is controlled below 1.5m.

[0038] The blocking sequence in step (3) is as follows: in the last furnace before the tundish stops casting, when the weighing shows that there are 25 tons of molten steel in the tundish, first block the 1st and 8th streams on both sides, and continue to cast the remaining 6 streams. Observe the length measuring instrument and block the flows in turn according to the actual length of the tail billet.

[0039] The continuous casting equipment with 8 machines and 8 streams uses a 60t tundish to hold about 55t of molten steel. When the molten steel in the tundish is 25t, the temperature of streams 1 and 8 on both sides is low. If the flow is not blocked in time, it will lead to failure to pull out. In addition, blocking the flow of streams 1 and 8 can change the flow path and direction of the molten steel, so that it can be more evenly distributed throughout the casting system. This can avoid the situation where there is too much or too little molten steel in a certain area, and reduce defects inside and on the surface of the ingot. At the same time, blocking the flow can also control the temperature and chemical composition distribution of the molten steel. By changing the flow and distribution of molten steel, the cooling rate and crystal structure of the molten steel can be better controlled, and the quality and performance of the ingot can be further optimized.

[0040] In step (4), the process of cooling first and then pulling down after the flow is blocked is that after the flow is blocked, the ingot is not pulled down directly, but is allowed to stay in the crystallizer for 10 seconds to cool and then pulled down.

[0041] By cooling for 10 seconds before the pull-down, the cooling time and quality of the billet can be increased, the surface quality of the billet and the density of the internal structure can be improved, and the shrinkage holes in the billet can be reduced. However, if the cooling time is too long, the billet may crack or change its structure due to excessive cooling. In addition, the adhesion between the billet and the crystallizer will increase, resulting in increased resistance to billet drawing, and even problems such as leakage and breakage. Through experiments on actual machines, the optimal cooling time before pull-down is 10 seconds, which can ensure the quality of the billet and the stability of production.

[0042] In step (5), the water content of the tail is controlled to be 1.2 L / kg, and the casting speed is automatically set to 2.5 m / min. After 2 minutes, the water content is adjusted to 1.0 L / kg, and the casting is automatically discharged at a speed of 2.0 m / min.

[0043] The control of water content and drawing speed during the tailing process is related to the quality of the tailing. Too little water content will lead to poor fluidity of molten iron, which is prone to defects such as insufficient pouring, slag inclusion, and pores. Too much water content will lead to excessive fluidity of molten iron and produce defects such as shrinkage, shrinkage, and cracks. At the same time, too high a drawing speed may cause defects such as cracks and looseness inside the ingot, while too low a drawing speed may cause defects such as cold shut and depression on the surface of the ingot. After repeated tests, the temperature of the molten steel is high in the early stage of tailing, and a large water content and high drawing speed should be used. The temperature of the molten steel is low in the later stage of tailing, and the water content and drawing speed need to be appropriately lowered.

[0044] The above-described embodiments are merely descriptions of preferred implementations of the present invention, and are not intended to limit the concept and scope of the present invention. Without departing from the design concept of the present invention, various modifications and improvements made by ordinary persons in the art to the technical solution of the present invention should all fall within the scope of protection of the present invention.

[0045] The techniques, shapes, and structural parts not described in detail in the present invention are all well-known techniques.

Claims

1. A method for controlling the length of the tail billet after stopping casting, characterized in that: The following steps are involved: (1) Increase the steel supply temperature of the stopped pouring furnace; (2) Block the flow according to the actual length of the tail billet; (3) Control the flow blocking sequence; (4) Cool down first and then pull down after blocking the flow; (5) Control the tail water volume; (6) After the tail is out, the flame cutting machine automatically cuts according to the normal fixed length; In step (1), the upper steel temperature of the stopped pouring furnace is increased from 1548°C to 1553°C. In step (2), the flow is blocked according to the actual length of the tail billet. A length measuring instrument is installed in the operation box of each flow to detect the position and length of the tail billet in real time, and the flow is blocked according to the actual length of the tail billet. The blocking sequence in step (3) is as follows: for the last furnace before the tundish stops casting, when the weighing shows that there are 25 tons of molten steel in the tundish, first block the 1st and 8th streams on both sides, and continue to cast the remaining 6 streams. Observe the length measuring instrument and block the streams in turn according to the actual length of the tail billet. The total capacity of the middle package is 60t; In step (4), cooling first and then pulling down after blocking the flow is that when the flow is blocked, it is not pulled down directly, but the billet is allowed to stay in the crystallizer for 10 seconds to cool and then pulled down; In step (5), the water content of the tail is controlled to be 1.2 L / kg when the tail is discharged. The casting speed is automatically set to 2.5 m / min. After 2 minutes, the water content is adjusted to 1.0 L / kg, and the casting is automatically discharged at a speed of 2.0 m / min.

Citation Information

Patent Citations

  • Method for pouring stopping of tundish of small square billets

    CN107649657A

  • Bearing steel continuous casting tail billet quality control method under unstable casting condition

    CN109648055A

  • Method for improving blank forming rate at casting last stage of continuous casting large-specification round blank

    CN116329509A

  • Process control method for reducing pouring residual steel of multi-machine multi-strand continuous casting tundish

    CN117139583A