A method for preparing sodium-enriched sodium vanadium phosphate / hard carbon composite positive electrode material
By using biomass-based hard carbon as a carrier, combined with ammonium metavanadate and ammonium dihydrogen phosphate, a sodium-rich sodium vanadium phosphate/hard carbon composite material was prepared, which solved the problem of poor energy density and rate performance of the sodium-ion battery cathode material. It achieves high energy density and excellent cycle stability, making it suitable for sodium-ion battery applications.
Patent Information
- Application Number
- CN202311603998.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-28
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-11-28
AI Technical Summary
Existing sodium-ion battery cathode materials have problems such as low energy density, low power density, and poor rate performance. Moreover, the existing methods of doping metal elements are complex and costly, making it difficult to effectively suppress the loss of sodium.
Biomass-based hard carbon is used as a sodium ion carrier, combined with ammonium metavanadate and ammonium dihydrogen phosphate to prepare nanoscale sodium vanadium phosphate/hard carbon composite cathode material. Through spray drying and staged calcination technology, sodium-enriched vanadium phosphate is achieved Preparation of sodium/hard carbon composite materials with high energy density and good cycle stability.
It achieves high electrochemical capacity and excellent rate performance of the sodium-ion battery cathode material, reduces the irreversible consumption of sodium ions, and the preparation process is simple, low-cost, environmentally friendly, and suitable for industrial production.
Smart Images

Figure CN117727885B_ABST
Abstract
Description
Technical Field
[0001] The present invention specifically relates to a method for preparing sodium-enriched sodium vanadium phosphate / hard carbon composite positive electrode material using biomass-based hard carbon as a carrier, which belongs to the positive electrode direction of sodium ion batteries in the field of sodium electric new energy material technology. Background Art
[0002] Biomass is the most abundant green energy on earth and is gaining more and more attention due to its low price and environmental protection. Biomass-derived carbon materials have great application potential in electrochemical energy storage systems due to their naturally existing layered structure to enhance the penetration of electrolytes and reduce the ion diffusion length. The raw materials of biomass-derived carbon are widely available and can be obtained from plants and animals, including bacteria, algae, herbs, agricultural waste, industrial waste, etc. In addition, a certain amount of N, O, and S extracted from biomass materials such as carbohydrates, proteins, and other organic macromolecules can form self-doped carbon materials with enhanced electrochemical properties.
[0003] Under the background of "dual carbon", the energy storage industry that matches clean energy has ushered in rapid development. Lead-acid batteries cause serious environmental pollution, and the reserves of lithium resources are also limited. Lithium-ion batteries are difficult to take into account the needs of the two major industries of electric vehicles and grid energy storage. Therefore, the demand for low-cost energy storage battery technology is becoming more and more urgent. Sodium-ion batteries are expected to be widely used in electric bicycles, low-speed electric vehicles, distributed energy storage and large-scale energy storage due to their advantages such as abundant sodium resources, low cost, good safety, excellent low-temperature performance, good fast charging performance, and high cost performance. However, a series of problems such as low energy density, low power density, and poor rate performance have become important reasons for restricting its large-scale development. The positive electrode material is the key to improving the performance of sodium-ion batteries, so it will be particularly important to develop sodium-ion battery positive electrode materials with excellent performance and low price.
[0004] The study found that sodium vanadium phosphate (Na 3 V 2 (PO 4 ) 3 , NVP) positive electrode material belongs to the hexagonal system, has the dual advantages of high rate performance and cycle performance, has two sodium ion migration channels, Na1 and Na2, and can provide a theoretical capacity of about 117 mAh / g. 3 V 2 (PO 4 ) 3This material shows that the sodium sites are not fully occupied in terms of structure, so it is actually possible to insert one more Na atom, and the problem of irreversible sodium consumption in sodium ion batteries can be effectively solved through positive electrode sodium compensation. However, it is difficult to introduce excess sodium into sodium vanadium phosphate by ordinary methods, and the loss of sodium cannot be effectively suppressed. Patent No. CN201811205129.0 discloses a method for preparing a sodium-rich sodium vanadium phosphate positive electrode material doped with metal manganese, which forms a P-type semiconductor by increasing the sodium content and adding a low-valent manganese element to replace the position of vanadium, thereby improving the electronic conductivity. Although this method reduces the use of vanadium to a certain extent, it does not solve the problem of sodium consumption from a macroscopic point of view. Patent No. CN202211046317.X also discloses a method for preparing a sodium-rich sodium vanadium phosphate positive electrode material doped with iron, manganese, and nickel metals. The invention also introduces sodium elements while doping low-valent metal elements, and acts together, and the obtained sodium vanadium phosphate is in a sodium-enriched state, thereby improving the performance of the positive electrode material. Although the above two methods reduce the use of vanadium to a certain extent, the operation of adding metal elements is complicated, the cost of the added metal is relatively high, and it also has a certain impact on resource consumption, which is not conducive to industrial production.
[0005] Biomass-based hard carbon is generally used as negative electrode material, but it has advantages such as versatility and microporosity, which can effectively improve the electrochemical performance of positive electrode materials for sodium ion batteries. Most biomass precursors have hierarchical porous structures and contain heteroatoms such as N, O, and S, which give biomass-derived carbon morphology inheritance and heteroatom self-doping characteristics. The sodium storage mechanism of hard carbon is generally recognized as the intercalation-filling model, adsorption-intercalation model, adsorption-filling model and third-order model. From the sodium storage mechanism, it can be seen that the sodium storage behavior of hard carbon mainly includes: (1) adsorption of heteroatoms, defects and functional groups; (2) embedding between carbon layers in graphite microcrystals; (3) filling in micropores. The porous structure of biomass-based hard carbon materials can provide channels for material transport and ion diffusion. Heteroatoms such as N and S can provide active sites for ion adsorption, improve material conductivity, and expand the distance between carbon layers.
[0006] By utilizing these properties of biomass-based hard carbon and using it as a carrier of sodium atoms to provide active sites for sodium ion adsorption, the positive electrode material is sodium-rich and the positive electrode material itself can accommodate more sodium, thereby solving the problem of irreversible sodium consumption in the positive electrode material of sodium ion batteries. The sodium-enriched sodium vanadium phosphate / hard carbon composite positive electrode material prepared by the present invention is expected to combine the advantages of sodium vanadium phosphate with a NASICON structure and hard carbon with a porous structure, thereby achieving higher battery capacity and better rate performance. Summary of the invention
[0007] In view of the requirements of the prior art for battery energy storage and cost, there is an urgent need for electrode materials with low cost and good performance, and there is no literature or patent reporting the application of biomass-based hard carbon in the preparation of sodium ion positive electrode materials. The present invention aims to provide a new method for preparing sodium vanadium phosphate / hard carbon composite positive electrode materials for sodium-rich sodium ion secondary batteries using biomass-based hard carbon as a carrier. The present invention uses ammonium metavanadate as a vanadium source, ammonium dihydrogen phosphate as a phosphorus source, and sodium carbonate as a sodium source to prepare a precursor, and uses biomass-based hard carbon as a carrier to obtain a nano-scale sodium vanadium phosphate material. No additional carbon source needs to be added during the material synthesis process. The preparation method is simple to operate, and the obtained material has high energy density, good crystallinity, and good electrochemical cycle stability. The preparation method of sodium vanadium phosphate / hard carbon composite positive electrode material provided by the present invention is an energy-saving, low-carbon, environmentally friendly, and economical green synthesis route, which does not pollute the environment and is easy to industrialize. It has good due value in sodium ion secondary batteries.
[0008] In order to achieve the above technical effects, the present invention provides the following solutions:
[0009] The present invention provides a sodium vanadium phosphate / hard carbon composite positive electrode material prepared using a biomass base as a sodium ion carrier, which has the following general formula:
[0010] Na 3+x V 2 (PO 4 ) 3 / C;
[0011] in, x It is 0.1-0.5.
[0012] The present invention also provides a method for preparing the above-mentioned sodium vanadium phosphate / hard carbon composite positive electrode material, and the specific process comprises the following steps:
[0013] (1) Preparation of biomass-based hard carbon material precursor: remove the biomass-based materials with mold spots by screening, wash and remove visible soil and impurities, put them in an oven to completely evaporate the water, then crush them and grind them into powder using a grinder. Transfer the powder to a reactor, pour KOH solution into it, and heat it continuously. After washing the obtained product to neutrality, put it into a beaker, and then pour H 2 SO 4 The solution is stirred in a constant temperature water bath until the product turns white. After washing to neutrality, the water is removed. The white product is placed in a zirconia ball milling jar, and the solvent is poured into the ball milling jar. After the solvent is dried, the biomass-based hard carbon material precursor is obtained.
[0014] (2) Preparation of sodium vanadium phosphate / hard carbon precursor: Add ammonium metavanadate and sodium carbonate into deionized water and stir until the ammonium metavanadate and sodium carbonate are completely dissolved to obtain a beige solution. Slowly add ammonium dihydrogen phosphate and stir until no obvious bubbles are generated in the solution. Then quickly add n-propanol and the biomass-based hard carbon material precursor described in (1), continue stirring to obtain a mixture, and then spray dry to obtain a sodium vanadium phosphate / hard carbon precursor.
[0015] (3) Preparation of sodium vanadium phosphate / hard carbon composite positive electrode material: Weigh the sodium vanadium phosphate / hard carbon precursor described in (2) in corundum, put it into a tube furnace for calcination, heat it under a protective atmosphere, and keep it warm for a period of time. After it naturally cools to room temperature, take it out, crush it with a powder grinder and mix it evenly, then pour the crushed powder solid into a sieve to sieve it, and obtain a high-performance sodium-rich sodium vanadium phosphate / hard carbon composite positive electrode material with uniform particle size distribution.
[0016] The biomass-based material provided by the present invention comprises one or more of walnut shells, peanut shells, corn stalks, chickpea shells, buckwheat shells, bagasse, lotus pods, and bamboo.
[0017] In the above technical solution, preferably, in step (1), the concentration of the KOH solution is 1-3 mol / L, the heating temperature is 100-120°C, the heating time is 12-14h, and H 2 SO 4 The concentration of the solution is 1-3 mol / L, and the temperature of the constant temperature water bath is 80-100℃.
[0018] In the above technical solution, preferably, in step (1), the solvent is one or more of methanol, ethanol, ether, deionized water, n-propanol, N,N-dimethylformamide, acetone, ethyl acetate, and petroleum ether.
[0019] In the above technical solution, preferably, in the step (1), the mass ratio of the white product to the zirconia balls is 1.10-1.50, and the diameter of the zirconia balls is 2-3 mm. In particular, low-speed pre-grinding can be adopted to make the materials mixed more evenly, with a pre-grinding speed of 100 r / min and a time of 1 h. After the pre-grinding is completed, the speed is adjusted to 400-1000 r / min and the ball milling is performed for 2-6 h.
[0020] In the above technical solution, preferably, in the step (2), the molar ratio of ammonium metavanadate, sodium carbonate and diammonium dihydrogen phosphate is 8-10:6-7:12-15, and the stirring temperature is 60-90°C.
[0021] In the above technical solution, preferably, in the step (2), the mass ratio of the biomass-based hard carbon material precursor to ammonium metavanadate is 1.5-2.0.
[0022] In the above technical solution, preferably, in step (2), the precursor material is spray dried by a spray dryer, a centrifugal spray dryer or a pressure spray dryer, the spray dryer inlet temperature is 200-350°C, and the spray drying outlet is 60-120°C. The spray drying fan is set to 75-95, the temperature is set to 160-250°C, the peristaltic pump is set to 10-50 mL / min, and the needle is set to 5-15 s. The particle size of the outlet particles can be precisely controlled by adjusting the solution solid content and the spray drying parameters, and the particle size range is 2-10 μm.
[0023] In the above technical solution, preferably, in step (3), the protective gas is argon, nitrogen, helium, neon or other inert gases, and the gas flow rate is 2-50 mL / min.
[0024] In the above technical solution, preferably, in the step (3), the heating rate is 2-10 °C / min. In particular, a staged calcination method can be used to fully increase the carbonization time. The heating rate of the first calcination is 2-10 °C / min, the first calcination temperature is 300-500 °C, the first calcination time is 2-5 h, and the heating rate of the second calcination is 2-10 °C / min, the second calcination temperature is 600-1000 °C, and the calcination time is 5-20 h.
[0025] In the above technical solution, preferably, in the step (3), the power of the powder mill is 200-2000 W, the working time does not exceed 30 s, the output particle size should be less than 0.5 mm, and the sieve mesh number is 200-350 mesh.
[0026] The main raw materials used in the present invention are rich in sources and low in price. No additional carbon source needs to be added during the synthesis process. The solubility of each substance is increased by heating and stirring in the precursor synthesis stage, and a certain amount of n-propanol is added to make each ion orderly combined in a microscopic state. The preparation method of the positive electrode material for sodium-rich sodium ion battery provided by the present invention has a simple and easy-to-operate preparation process. Biomass-based hard carbon can be obtained while obtaining the positive electrode material, thereby having multiple sodium storage methods. The obtained sodium vanadium phosphate / hard carbon composite positive electrode material has high electrochemical capacity and good cycle stability, and has good application value in sodium ion secondary batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is the XRD diagram of the sodium vanadium phosphate / hard carbon composite material synthesized by the preparation method described in Example 1.
[0028] Figure 2 This is a particle size diagram of the sodium vanadium phosphate / hard carbon composite material synthesized by the preparation method described in Example 1.
[0029] Figure 3 This is a SEM image of the sodium vanadium phosphate / hard carbon composite material synthesized by the preparation method described in Example 1.
[0030] Figure 4 This is a charge and discharge curve diagram of the first week of the sodium vanadium phosphate / hard carbon composite material synthesized by the preparation method described in Example 1 at a current density of 0.1C.
[0031] Figure 5 This is a cycle curve diagram of the sodium vanadium phosphate / hard carbon composite material synthesized by the preparation method described in Example 1 at a 2 C current density. DETAILED DESCRIPTION
[0032] In order to better understand the present invention, the content of the present invention is further described below in conjunction with embodiments and related drawings, but the content of the present invention is not limited to the following embodiments.
[0033] This embodiment provides a method for preparing a sodium-enriched sodium vanadium phosphate / hard carbon composite positive electrode material using biomass-based hard carbon as a sodium ion carrier, and the specific steps are:
[0034] (1) Preparation of biomass-based hard carbon material precursor: Screen and remove biomass-based materials with mold spots, wash and remove visible soil and impurities, put them in an oven to completely evaporate the water, then crush them and grind them into powder using a grinder. Transfer the powder to a reactor, pour 1-3 mol / L KOH solution into it, and heat it continuously at 100 °C for 10-20 h. After the obtained product is washed to neutrality, put it into a beaker, and then pour 1-3 mol / L H 2 SO 4 The solution was stirred in a constant temperature water bath at 80 °C until the product turned white, washed to neutrality and then the water was removed. The white product was placed in a zirconia ball milling jar, the mass ratio of the white product to the zirconia ball was 1.10-1.50, the diameter of the zirconia ball was 2-3 mm, 50 mL of solvent was poured in, pre-milled at 100 r / min for 1 h, the speed was adjusted to 400-1000 r / min, ball milled for 2-6 h, and the biomass-based hard carbon material precursor was obtained after the solvent was dried.
[0035] (2) Preparation of sodium vanadium phosphate / hard carbon precursor: 8 mmol of ammonium metavanadate and 6.2-7 mmol of sodium carbonate were added to deionized water, stirred at 60-90 °C until the ammonium metavanadate and sodium carbonate were completely dissolved to obtain a beige solution, 12 mmol of ammonium dihydrogen phosphate was slowly added, stirred until no obvious bubbles were generated in the solution, and then 50 mL of n-propanol and 1.42-1.89 g of the biomass-based hard carbon material precursor described in (1) were quickly added, and stirring was continued for 20 min to obtain a mixture. The spray dryer inlet temperature was 200-350 °C, and the spray dryer outlet was 60-120 °C. The spray dryer fan was set to 75-95, the temperature was set to 160-250 °C, the peristaltic pump was set to 10-50 mL / min, and the needle was set to 5-15 s. Spray drying was performed to obtain a sodium vanadium phosphate / hard carbon precursor.
[0036] (3) Preparation of sodium vanadium phosphate / hard carbon composite positive electrode material: Weigh the sodium vanadium phosphate / hard carbon precursor described in (2) in corundum and place it in a tube furnace for calcination. Under a protective atmosphere, the heating rate of the first calcination is 2-10 °C / min, the temperature is 300-500 °C, and the time is 2-5 h. The heating rate of the second calcination is 2-10 °C / min, the temperature is 600-1000 °C, and the time is 5-20 h. After waiting for it to naturally cool to room temperature, take it out, crush it with a powder grinder and mix it thoroughly. The power of the powder grinder is 200-2000W, and the working time does not exceed 30 s. Then pour the crushed powdered solid into a sieve and sieve it with a mesh size of 200-350 to obtain a high-performance sodium-rich sodium vanadium phosphate / hard carbon composite positive electrode material with uniform particle size distribution.
[0037] Example 1
[0038] Based on the above implementation, this embodiment provides a method for preparing sodium-enriched sodium vanadium phosphate / hard carbon composite positive electrode material using biomass-based hard carbon as a sodium ion carrier. The specific steps are as follows: (1) Preparation of biomass-based hard carbon material precursor: the concentration of KOH solution is 1 mol / L, the heating time is 16 h, and H 2 SO 4The concentration of the solution was 1 mol / L. The mass ratio of the mixed material to the zirconia ball was 1.10, the diameter of the zirconia ball was 2 mm, the rotation speed was 400 r / min, and the ball milling time was 4 h. (2) Preparation of sodium vanadium phosphate / hard carbon material precursor: ammonium metavanadate was 8 mmol, sodium carbonate was 6.2 mmol, the stirring temperature was 90 °C, diammonium phosphate was 12 mmol, and the biomass-based hard carbon material precursor was 1.42 g. The precursor material was spray dried using a spray dryer. The inlet temperature of the spray dryer was 280 °C and the outlet temperature of the spray dryer was 95 °C. The spray drying fan was set to 90, the temperature was set to 180 °C, the peristaltic pump was set to 20 mL / min, and the needle was set to 10 s. (3) Preparation of sodium vanadium phosphate / carbon composite positive electrode material: The protective atmosphere was nitrogen, the heating rate of the first calcination was 3 °C / min, the temperature was 600 °C, and the time was 2 h. The heating rate of the second calcination was 5 °C / min, the temperature was 900 °C, and the time was 10 h. The power of the powder machine was 1000 W, the working time was 20 s, and the sieve size was 350 mesh. EDX analysis showed that the final Na 3.1 V 2 (PO 4 ) 3 / C positive electrode material.
[0039] Example 2
[0040] The difference between Example 2 and Example 1 is that the concentration of KOH solution is 2 mol / L; the heating time is 14 h; H 2 SO 4 The concentration of the solution was 2 mol / L; the mass ratio of the mixed material to the zirconia ball was 1.20; the diameter of the zirconia ball was 3 mm, the rotation speed was 600 r / min, and the ball milling time was 6 h; the sodium carbonate content was 6.4 mmol; and the biomass-based hard carbon material precursor was 1.51 g. EDX analysis showed that the final Na 3.2 V 2 (PO 4 ) 3 / C positive electrode material.
[0041] Example 3
[0042] The difference between Example 3 and Example 2 is that the concentration of KOH solution is 3 mol / L; the heating time is 12 h; H 2 SO 4 The concentration of the solution is 3 mol / L; the sodium carbonate is 6.6 mmol; and the biomass-based hard carbon material precursor is 1.61 g. EDX analysis shows that the final Na 3.3 V 2 (PO 4 ) 3 / C positive electrode material.
[0043] Example 4
[0044] The difference between Example 4 and Example 2 is that the sodium carbonate is 6.8 mmol and the biomass-based hard carbon material precursor is 1.70 g. EDX analysis shows that the final Na 3.4 V 2 (PO 4 ) 3 / C positive electrode material.
[0045] Example 5
[0046] The difference between Example 5 and Example 2 is that the sodium carbonate is 7.0 mmol and the biomass-based hard carbon material precursor is 1.80 g. EDX analysis shows that the final Na 3.5 V 2 (PO 4 ) 3 / C positive electrode material.
[0047] Comparative Example 1
[0048] The difference between Comparative Example 1 and Example 2 is that no carbon source is used as the carbon coating material. EDX analysis shows that the final Na 3 V 2 (PO 4 ) 3 Positive electrode material.
[0049] Table 1 shows the battery performance of sodium vanadium phosphate / hard carbon composite positive electrode materials prepared in Examples 1-5 and Comparative Example 1
[0050]
[0051] As can be seen from Table 1, when Na:V:P is 3.5:2:3 in Example 5, the discharge capacity of the sodium vanadium phosphate positive electrode material at a current density of 0.1 C is the highest, which is 119.3 mAh / g. When the sodium vanadium phosphate positive electrode material is not carbon-coated, Na:V:P is 3:2:3, sodium ions are lost to a certain extent in the positive electrode material, and the discharge capacity at a current density of 0.1 C is 95.1 mAh / g, which is lower than the battery performance after adding hard carbon as a carbon coating material. It can be seen that adding hard carbon as a carbon source has the effect of reducing the irreversible loss of sodium ions, making the positive electrode material sodium-enriched, and significantly improving the discharge capacity and rate performance of the battery.
[0052] By the attached Figure 1The data show that the sodium vanadium phosphate / hard carbon composite positive electrode material obtained by the present invention has no obvious impurity peaks compared with the standard card, and has good crystallinity. When the calcination temperature is 900°C and the calcination time is 10 h, the obtained sodium vanadium phosphate / hard carbon composite positive electrode material has the best crystallinity.
[0053] By the attached Figure 2 The data show that the D50 of the sodium vanadium phosphate / hard carbon composite positive electrode material obtained in the present invention is 6.710 μm. The particle size of the sodium vanadium phosphate / hard carbon composite positive electrode material obtained in the present invention is controlled between 2-10 μm.
[0054] By the attached Figure 3 The data show that the sodium vanadium phosphate / hard carbon composite positive electrode material obtained in the present invention is a fluffy, porous block inside, which contains a huge space for storing sodium atoms, which is not only beneficial to the infiltration of the electrode liquid, but also to the deintercalation of sodium ions.
[0055] By the attached Figure 4 The data show that the sodium vanadium phosphate / carbon composite positive electrode material obtained in the present invention has a discharge specific capacity of 112.4 mAh / g at a current density of 0.1 C, and a 1 C / 0.2 C rate performance of 98.3%, showing excellent electrochemical performance.
[0056] By the attached Figure 5 From the data, we can see that the cycle performance diagram at 2 C current density shows that after 90 cycles, the capacity retention rate is still 96%, and the material exhibits excellent cycle performance.
[0057] From the above data, it can be seen that the preparation method of the sodium-rich sodium ion battery positive electrode material provided by the present invention has a simple preparation process and is easy to operate. While obtaining the positive electrode material, biomass-based hard carbon can be obtained; no additional carbon source needs to be added during the material synthesis process, and the obtained sodium-rich sodium vanadium phosphate / hard carbon composite positive electrode material has good crystallinity, high electrochemical capacity, and good cycle stability, and has great application value in sodium ion secondary batteries.
[0058] It should be understood that the above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a sodium-rich sodium vanadium phosphate / hard carbon composite positive electrode material, characterized in that: Acid-base pretreatment of biomass-based materials to obtain a precursor specifically includes the following steps: (1) Preparation of biomass-based hard carbon material precursor: The biomass-based material is heated and impregnated with a KOH solution, then heated and stirred in a H2SO4 solution in a water bath, washed until neutral, and then ball-milled with a solvent to obtain a biomass-based hard carbon material precursor. The concentration of the KOH solution is 1-3 mol / L, the heating temperature is 100-120°C, the heating time is 12-14h, the concentration of the H2SO4 solution is 1-3 mol / L, and the constant temperature water bath temperature is 80-100°C; (2) Preparation of sodium vanadium phosphate / hard carbon precursor: ammonium metavanadate and sodium carbonate solution are mixed, and ammonium dihydrogen phosphate is added under stirring, followed by rapid addition of n-propanol and the biomass-based hard carbon material precursor described in step (1), and stirring is continued to obtain a mixture, which is then spray-dried to obtain a sodium vanadium phosphate / hard carbon precursor, wherein the mass ratio of the biomass-based hard carbon material precursor to the ammonium metavanadate is 1.5-2.0; (3) Preparation of sodium vanadium phosphate / hard carbon composite positive electrode material: The sodium vanadium phosphate / hard carbon precursor described in (2) is weighed and calcined to obtain a sodium-rich sodium vanadium phosphate / hard carbon composite positive electrode material. The sodium-rich sodium vanadium phosphate / hard carbon composite positive electrode material has the following general formula: Na 3+x V2(PO4)3 / C; where x It is 0.1-0.
5.
2. The method for preparing the sodium-rich sodium vanadium phosphate / hard carbon composite positive electrode material according to claim 1, characterized in that: Biomass-based materials include walnut shells, peanut shells, corn stalks, chickpea shells, buckwheat husks, bagasse, lotus pods or bamboo.
3. The method for preparing the sodium-rich sodium vanadium phosphate / hard carbon composite positive electrode material according to claim 1, characterized in that: The solvent in step (1) is selected from one or more of methanol, ethanol, ether, deionized water, n-propanol, N,N-dimethylformamide, acetone, ethyl acetate, and petroleum ether.
4. The method for preparing the sodium-rich sodium vanadium phosphate / hard carbon composite positive electrode material according to claim 1, characterized in that: In the step (2), the molar ratio of ammonium metavanadate, sodium carbonate and diammonium dihydrogen phosphate is 8-10:6-7:12-15, and the stirring temperature is 60-90°C.
5. The method for preparing the sodium-rich sodium vanadium phosphate / hard carbon composite positive electrode material according to claim 1, characterized in that: The particle size range achieved after spray drying in step (2) is 2-10 μm.
6. The method for preparing the sodium-rich sodium vanadium phosphate / hard carbon composite positive electrode material according to claim 1, characterized in that: In the step (3), the protective gas is argon, nitrogen, helium or neon, and the gas flow rate is 2-50 mL / min; the carbonization time is fully increased by adopting a staged calcination method, the heating rate of the first calcination is 2-10°C / min, the first calcination temperature is 300-500°C, the first calcination time is 2-5 h, the heating rate of the second calcination is 2-10°C / min, the second calcination temperature is 600-1000°C, and the calcination time is 5-20 h.
7. The method for preparing the sodium-rich sodium vanadium phosphate / hard carbon composite positive electrode material according to claim 1, characterized in that: Step (3) also includes waiting for the mixture to naturally cool to room temperature before taking it out and crushing it with a powder grinder. The power of the powder grinder is 200-2000 W, the working time is 1-30 s, the particle size of the output is 0.1-0.5 mm, and the sieve mesh number is 200-350 meshes.