A positively charged hollow fiber nanofiltration membrane and its preparation method and application

By using the reaction of γ-glycidyl etheroxypropyl trimethoxysilane oligomer with amine compounds in the interfacial polymerization method of hollow fiber nanofiltration membrane, combined with the double-layer spinneret technology, a positive-charge selective layer is formed. The problems of structural instability and low cation removal efficiency of hollow fiber nanofiltration membranes in the prior art are solved, and efficient salt retention and water treatment effects are achieved.

CN117732270BActive Publication Date: 2024-11-08SUN YAT SEN UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410105096.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-24
Publication Date
2024-11-08
Estimated Expiration
2044-01-24

AI Technical Summary

Technical Problem

During the preparation process of the existing hollow fiber nanofiltration membrane, there are problems such as uneven monomer distribution, unstable nanofiltration layer structure, inability to pressurize backflush and impermissible chlorine resistance, and spinning treated with single-hole spinneret The polymer cast film liquid cannot control the cortex and support layer separately, resulting in difficulty in reducing the pore size and low cation removal efficiency.

Method used

The γ-glycidyl etheroxypropyl trimethoxysilane oligomer was used as an additive, reacted with amine compounds, and extruded by double-layer spinnerets to prepare an external pressure hollow fiber membrane to form a dense positive-charge selective layer. The removal of cations is achieved and a network structure is formed by hydrolysis reaction under acidic conditions to enhance the flux and retention of the membrane.

Benefits of technology

The prepared positive-charged hollow fiber nanofiltration membrane has a low average molecular retention and a high salt retention rate, maintains a good flux, and shows excellent removal performance in wastewater, wastewater and drinking water treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117732270B_ABST
    Figure CN117732270B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a positively charged hollow fiber nanofiltration membrane. The preparation method comprises the following steps: S1. mixing an oligomer additive with a polymer, adding a pore-forming agent and a solvent, and preparing an outer layer spinning casting solution; S2. preparing an inner layer spinning casting solution; S3. preparing a spinning core solution; S4. extruding the outer layer spinning casting solution, the inner layer spinning casting solution and the spinning core solution through a double-layer spinneret to prepare an external pressure type hollow fiber membrane; S5. immersing the external pressure type hollow fiber membrane in an amine compound solution for cross-linking modification to obtain a positively charged hollow fiber nanofiltration membrane. The positively charged external pressure type hollow fiber nanofiltration membrane prepared by the present invention comprises a double-layer membrane structure consisting of a positively charged dense cortex and a porous support layer, which can achieve the removal of cations, and has a lower average molecular retention and a higher salt retention rate, maintaining a better flux.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of separation membranes, and more specifically, relates to a positively charged hollow fiber nanofiltration membrane and a preparation method and application thereof. Background Art

[0002] As an emerging water treatment technology, membrane separation technology has been rapidly developed and widely used in the past two decades due to its advantages such as small footprint, high treatment efficiency and good effluent quality. Among them, nanofiltration technology is a low-pressure driven membrane separation technology with a pore size between ultrafiltration and reverse osmosis (0.5-2nm). It can effectively intercept small organic molecules such as dyes, humus, micropollutants and multivalent inorganic ions in water bodies, and has been widely used in drinking water purification, industrial wastewater reuse, water softening, seawater desalination and other fields. At present, most commercial nanofiltration membrane components on the market are roll-type membrane components composed of flat membranes, which have problems such as low unit membrane component filling density, high operating pressure (>5bar) required to produce water, easy concentration polarization, water inlet pretreatment, difficulty in backwashing, secondary pollution risk and chlorine resistance. In addition, frequent replacement of membrane components caused by membrane pollution will also lead to high investment and operating costs. Therefore, the development of new nanofiltration membranes or membrane component configurations is the key to solving the problem.

[0003] Compared with traditional rolled membranes, hollow fiber nanofiltration membranes have a self-supporting structure, unlike flat membranes that require non-woven fabrics for support. In addition, hollow fiber membrane components do not require separators on the water inlet and permeate sides, and have high unit component filling density and large water production. The hydraulic conditions on the inner and outer surfaces of the hollow fiber membrane can be improved by controlling the flow rate, which can effectively overcome concentration polarization, reduce head loss, and thereby reduce operating pressure and membrane pollution. In addition, hollow fiber membrane components can also be backwashed. At the same time, the hollow fiber nanofiltration membrane prepared based on the phase inversion method has good chlorine resistance and can be cleaned with sodium hypochlorite.

[0004] At present, the preparation methods of hollow fiber nanofiltration membranes mainly include phase inversion method, interfacial polymerization method and polyelectrolyte layer-by-layer self-assembly coating method. Chinese patent CN202210047226.1 alcoholizes the existing hollow fiber ultrafiltration membrane and then soaks it in polyamine, and obtains a hollow fiber composite nanofiltration membrane by interfacial polymerization. However, during the interfacial polymerization process, the water phase is prone to uneven distribution on the outer surface of the membrane fiber, which makes the prepared nanofiltration membrane separation layer have obvious deficiencies in integrity and stability. In addition, the composite membrane prepared by interfacial polymerization still cannot be backwashed under pressure due to the weak interaction between polyamide and the base membrane, and is not chlorine-resistant. Compared with the interfacial polymerization method, the phase inversion method solves the problem of uneven monomer distribution in the interfacial polymerization method, thereby making the nanofiltration layer structure more stable and complete. The literature [Thong Z, Gao J, Lim JXZ, et al. Fabrication of loose outer-selective nanofiltration (NF) polyethersulfone (PES) hollow fibers via single-step spinning process for dye removal [J]. Separation and Purification Technology, 2018, 192 (483-90)] uses a single-hole spinneret to prepare a polyethersulfone hollow fiber nanofiltration membrane through a dry-wet spinning process, with an average molecular weight cutoff (MWCO) of 1500 Da. However, there is only one type of spinning polymer casting solution processed by a single-hole spinneret, and it is impossible to achieve separate regulation of the cortex and the support layer. The pore size of the prepared nanofiltration membrane is difficult to further reduce, and the water resistance is often large; and more importantly, the surface of the prepared nanofiltration membrane is usually negatively charged, which cannot achieve the removal of cations. Summary of the invention

[0005] In view of the above-mentioned existing technical problems, the primary purpose of the present invention is to provide a method for preparing a positively charged hollow fiber nanofiltration membrane, which uses γ-glycidyloxypropyltrimethoxysilane oligomer as a reaction additive and can react with amine compounds. The prepared positively charged external pressure hollow fiber nanofiltration membrane can remove cations and has a lower average molecular retention capacity and a higher salt retention rate, thereby maintaining a better flux.

[0006] The second object of the present invention is to provide a positively charged hollow fiber nanofiltration membrane prepared by the above-mentioned method for preparing the positively charged hollow fiber nanofiltration membrane.

[0007] The third object of the present invention is to provide the application of the positively charged hollow fiber nanofiltration membrane in the fields of sewage treatment, wastewater treatment, seawater desalination, and drinking water treatment.

[0008] In order to achieve the above object, the present invention is implemented through the following technical solutions.

[0009] A method for preparing a positively charged hollow fiber nanofiltration membrane comprises the following steps:

[0010] S1. The γ-glycidyl ether oxypropyl trimethoxysilane oligomer additive is mixed with a polymer, a pore-forming agent and a solvent are added to prepare a hollow fiber membrane outer layer spinning casting solution;

[0011] The structural formula of the γ-glycidyloxypropyltrimethoxysilane oligomer additive is as follows:

[0012] Wherein, n is 5 to 13;

[0013] S2. Mixing a polymer, a pore-forming agent and a solvent to prepare a hollow fiber membrane inner layer spinning casting solution; in the steps S1 and S2, the polymer is selected from one or more of polyethersulfone, polysulfone and polyvinylidene fluoride;

[0014] S3. preparing a spinning core solution;

[0015] S4. Extruding the outer layer spinning casting solution, the inner layer spinning casting solution and the spinning core solution of the hollow fiber membrane through a double-layer spinneret to prepare an external pressure hollow fiber membrane;

[0016] S5. The external pressure hollow fiber membrane is immersed in an amine compound solution for cross-linking modification and post-treatment to obtain the positively charged hollow fiber nanofiltration membrane.

[0017] The inventor first prepared γ-glycidyloxypropyltrimethoxysilane oligomer under acidic conditions, which can be used as a new additive in the casting solution. The inventor found through research that the oligomer additive formed by hydrolysis and polycondensation under acidic conditions is easy to form a network structure, and the oligomer with a network structure has good compatibility with the polymer. However, the oligomer prepared by hydrolysis under alkaline conditions will form a three-dimensional gel structure, which is incompatible with the polymer, cannot be used as an additive, and cannot be prepared by spinning. Secondly, when the molecular weight of the oligomer is small, on the one hand, the oligomer with a small molecular weight is easy to dissolve during the film formation process, and a hollow fiber membrane with reactive surface cannot be constructed; on the other hand, the prepared hollow fiber membrane has a relatively high flux, but the retention rate is very low, and it is not even within the range of nanofiltration.

[0018] Furthermore, the γ-glycidyloxypropyltrimethoxysilane oligomer carries an active reactive group (epoxy group). During the phase inversion process, due to the hydrophilicity of the silanol chain segment, it can migrate to the surface of the membrane during the solvent-nonsolvent exchange process, thereby forming a silane cross-linked network on the surface of the hollow fiber membrane, enhancing the hydrophilicity and reactivity of the membrane, and thus improving the flux, retention rate and average molecular weight cutoff of the membrane. In addition, the surface of the γ-glycidyloxypropyltrimethoxysilane oligomer contains abundant epoxy groups, which have high reactivity with amine polymers, so that a dense positively charged selective layer is formed on the surface of the hollow fiber membrane, thereby achieving the removal of cations.

[0019] The present invention adopts a double-layer spinneret to extrude the casting liquid. Compared with spinning with a single-hole spinneret, the double-hole spinneret is used to spin a double-layer hollow fiber membrane, and the components of the inner and outer casting liquids can be respectively regulated to prepare a hollow fiber membrane with a double-layer structure of a dense skin layer and a porous support layer, thereby obtaining an external pressure type hollow fiber nanofiltration membrane with higher flux and smaller pore size (the pure water flux of the external pressure type hollow fiber nanofiltration membrane spun by the single-hole spinneret is 8.5LMH / bar, and the retention rate of PEG2000 is 64.3%; while the pure water flux of the external pressure type hollow fiber nanofiltration membrane spun by the double-hole spinneret is 17.7LMH / bar, and the retention rate of PEG2000 is 75.4%).

[0020] Preferably, the preparation method of the γ-glycidyloxypropyltrimethoxysilane oligomer additive is: under acidic conditions, γ-glycidyloxypropyltrimethoxysilane, alcohol solvent and pure water are mixed, heated and stirred, and the solvent is removed to obtain the γ-glycidyloxypropyltrimethoxysilane oligomer additive.

[0021] Preferably, the heating and stirring time is 12 to 48 hours. Further preferably, the heating and stirring time is 12 to 36 hours. The inventors have found through research that within a certain reaction time range, the molecular weight of the oligomer additive increases with the increase of the reaction time; when the reaction time exceeds 72 hours, the oligomer additive obtained by the reaction undergoes reverse decomposition, which is not conducive to the preparation of the oligomer additive. When the reaction time is insufficient, the molecular weight of the prepared oligomer is too small, and it is easy to dissolve in the subsequent membrane formation process, and it is impossible to construct a hollow fiber membrane with reactive surface.

[0022] Preferably, the acidic condition is achieved by adding an acid auxiliary agent; the acid auxiliary agent may be concentrated sulfuric acid, etc. Preferably, the mass ratio of the γ-glycidyloxypropyltrimethoxysilane oligomer to the catalyst concentrated hydrochloric acid is 25:1-10.

[0023] Preferably, the alcohol solvent is a mixed solvent of methanol and ethanol, wherein the volume proportion of methanol is 20-80%.

[0024] Preferably, the heating temperature is 50-80°C.

[0025] Preferably, the solvent is evaporated off by vacuum evaporation at 50-80° C. in a water bath for 1-2 h.

[0026] Preferably, the outer layer spinning casting solution of the hollow fiber membrane comprises, by mass percentage, 1 to 10% γ-glycidyl ether oxypropyl trimethoxy silane oligomer additive, 24 to 32% polymer, 1 to 10% pore former, and the balance is solvent. Further preferably, the outer layer spinning casting solution of the hollow fiber membrane comprises: 4 to 6% γ-glycidyl ether oxypropyl trimethoxy silane oligomer additive, 24 to 32% polymer, 1 to 10% pore former, and the balance is solvent.

[0027] Preferably, the preparation method of the outer layer spinning casting liquid of the hollow fiber membrane is: under sealed conditions, the above substances are stirred in a constant temperature water bath of 50-80°C for 6-12 hours, stirring is stopped after they are completely dissolved, and the mixture is allowed to stand and vacuumed for degassing to obtain the outer layer spinning casting liquid of the hollow fiber membrane.

[0028] Preferably, the inner layer spinning casting solution of the hollow fiber membrane comprises, by mass percentage, 10-24% polymer, 10-40% pore former, and the balance is solvent. Further preferably, the inner layer spinning casting solution of the hollow fiber membrane comprises, by mass percentage, 18-22% polymer, 35-40% pore former, and the balance is solvent.

[0029] Preferably, the preparation method of the inner layer spinning casting liquid of the hollow fiber membrane is: under sealed conditions, the above substances are stirred in a constant temperature water bath of 50-80°C for 6-12 hours, stirring is stopped after they are completely dissolved, and the mixture is allowed to stand and vacuumed for degassing to obtain the inner layer spinning casting liquid of the hollow fiber membrane.

[0030] Preferably, the hollow fiber membrane spinning core liquid is a mixed solution of solvent and / or water.

[0031] Preferably, the amine compound is selected from one or more of polyethyleneimine, polyallylamine hydrochloride, polyacrylamine, ethylenediamine, and hexamethylenediamine. Further preferably, the amine compound is polyethyleneimine.

[0032] Preferably, the molecular weight of the amine compound is 600 to 70,000 Da. Further preferably, the molecular weight of the amine compound is 20,000 to 30,000 Da. Under this preferred condition, the positively charged hollow fiber nanofiltration membrane has a lower average molecular weight cutoff and a higher salt retention rate.

[0033] Preferably, the mass concentration of the amine compound solution is 1-5%.

[0034] Preferably, the solvent is selected from one or more of dimethyl sulfoxide, dimethylformamide, dimethylacetamide and N-methylpyrrolidone.

[0035] Preferably, the pore-forming agent can be selected from conventional pore-forming agents in the art. More specifically, the pore-forming agent can be selected from one or more of polyvinyl pyrrolidone, polyethylene glycol, lithium chloride, and lithium fluoride. More specifically, the pore-forming agent can be polyvinyl pyrrolidone, and its molecular weight can be 8000 to 700000 Da; the pore-forming agent can be polyethylene glycol, and its molecular weight can be 200 to 20000 Da.

[0036] Preferably, in some specific embodiments, a dry-wet spinning process is used to prepare an external pressure hollow fiber membrane. The specific operation of the dry-wet spinning process is: the outer layer spinning casting liquid and the inner layer spinning casting liquid of the hollow fiber membrane are filtered, and then the outer layer spinning casting liquid and the inner layer spinning casting liquid of the hollow fiber membrane are extruded from the outer ring and the inner ring of the double-layer spinneret respectively at the same time, and the hollow fiber membrane spinning core liquid is ejected from the center of the spinneret, and the collection speed is controlled by the collection wheel; after a certain air gap, the primary hollow fiber enters the coagulation bath and undergoes phase transformation, and is soaked in pure water to obtain an external pressure hollow fiber membrane.

[0037] Preferably, the spinning pressure during the extrusion is 0.1-0.4 MPa.

[0038] Preferably, the extrusion flow rate is 5 to 15 g / min.

[0039] Preferably, the flow rate of the hollow fiber membrane spinning core liquid is 5 to 10 g / min.

[0040] Preferably, the length of the air gap is 0.5-15 cm.

[0041] Preferably, the temperature of the coagulation bath is 10-60°C.

[0042] Preferably, the wire collecting wheel has a wire collecting speed of 5-20 m / min.

[0043] Preferably, the pure water immersion time is 24 to 72 hours.

[0044] Preferably, the cross-linking modification is carried out under heating conditions of 40 to 70° C. in a water bath for 1 to 4 hours.

[0045] Preferably, the post-treatment is: soaking the cross-linked modified membrane in pure water, then taking out the membrane fibers and soaking them in an aqueous solution containing glycerol, and drying them to obtain a positively charged hollow fiber nanofiltration membrane.

[0046] Furthermore, the present invention seeks to protect a method for preparing a positively charged hollow fiber nanofiltration membrane and a positively charged hollow fiber nanofiltration membrane obtained by the preparation.

[0047] Furthermore, the present invention seeks to protect the application of positively charged hollow fiber nanofiltration membrane in the fields of sewage treatment, wastewater treatment, seawater desalination, and drinking water treatment.

[0048] Compared with the prior art, the present invention has the following beneficial effects:

[0049] The present invention provides a method for preparing a positively charged hollow fiber nanofiltration membrane. A double-layer spinneret is used to extrude the casting solution, and the components of the inner and outer casting solutions can be respectively regulated to prepare a hollow fiber membrane with a double-layer structure of a dense skin layer and a porous support layer. By adding a γ-glycidyloxypropyltrimethoxysilane oligomer additive in the reaction, the surface of which contains abundant epoxy groups and has high reactivity with amine polymers, a dense positively charged selective layer is formed on the surface of the hollow fiber membrane, thereby achieving the removal of cations. The positively charged hollow fiber nanofiltration membrane prepared by the present invention has a lower average molecular retention and a higher salt retention rate, and maintains a good flux. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figure 1 The outer surface morphology of the hollow fiber membranes prepared in Examples 1-3 and Comparative Examples 1-4.

[0051] Figure 2 The cross-sectional morphology of the hollow fiber membranes prepared in Comparative Examples 1-4.

[0052] Figure 3 The cross-sectional morphology diagrams of the hollow fiber membranes prepared in Examples 1-3 and Comparative Example 3.

[0053] Figure 4 These are the surface charge test results of the hollow fiber membranes prepared in Examples 1-3 and Comparative Examples 1-4.

[0054] Figure 5 The distribution results of oligomer molecular weight at different reaction times. DETAILED DESCRIPTION

[0055] The present invention is further described below in conjunction with the accompanying drawings and specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0056] Example 1 Preparation of a positively charged hollow fiber nanofiltration membrane

[0057] (1) Preparation of γ-glycidyloxypropyltrimethoxysilane oligomer

[0058] Dissolve 25g of γ-glycidyloxypropyltrimethoxysilane in 60ml of a mixed solvent of methanol and ethanol, with methanol accounting for 67% by volume, add 19.9ml of pure water as a hydrolysis reactant, and add 8.1g of concentrated hydrochloric acid as a catalyst. React in an oil bath at 65°C under magnetic stirring for 24 hours. The solution after the reaction is evaporated with a rotary evaporator to obtain γ-glycidyloxypropyltrimethoxysilane oligomer.

[0059] (2) Configuration of spinning casting solution

[0060] The outer layer casting solution is prepared by blending the oligomer obtained in step (1) with polyethersulfone, wherein the mass percentage of the oligomer is 5%, the mass percentage of the polyethersulfone is 30%, the mass percentage of the pore former (polyvinyl pyrrolidone) is 1%, and the solvent is N-methylpyrrolidone. The above substances are added to a sealed glass reaction dish, and mechanically stirred in a 60°C constant temperature water bath for 8 hours. After the mixture is completely dissolved, stirring is stopped, and the mixture is allowed to stand for 3 hours to be vacuumed and degassed, thereby obtaining the outer layer spinning casting solution.

[0061] The configuration of the inner layer casting solution: the mass percentage of polyethersulfone is 20%, the mass percentage of pore former (polyethylene glycol) is 40%, and the solvent is N-methylpyrrolidone. The above substances are added to a sealed glass reaction dish, mechanically stirred in a 60°C constant temperature water bath for 8 hours, and the stirring is stopped after the complete dissolution, and the solution is allowed to stand for 3 hours to be vacuumed and degassed, thereby obtaining the inner layer spinning casting solution.

[0062] Preparation of core liquid: Mix pure water and N-methylpyrrolidone in a beaker to prepare 500 ml solution (of which pure water accounts for 20%). After mixing, stir the solution in a 25°C water bath for 30 minutes until the temperature is constant to obtain the required core liquid.

[0063] (3) Preparation of external pressure hollow fiber membrane

[0064] The spinning casting liquid was filtered with a stainless steel filter head. Under a spinning pressure of 0.2MPa, the outer casting liquid was extruded from the outer ring of the double-hole spinneret at a flow rate of 9g / min, the inner casting liquid was extruded from the inner ring of the double-hole spinneret at a flow rate of 6g / min, and the core liquid was ejected from the core liquid flow channel at a flow rate of 5g / min; the primary hollow fiber passed through an air gap of 0.5cm, solidified in pure water at a temperature of 20°C, wound at a speed of 9m / min, and then soaked in pure water for 24h to obtain an external pressure hollow fiber membrane.

[0065] (4) Cross-linking modification of external pressure hollow fiber membrane

[0066] The membrane fibers were immersed in a sealed container containing 2% polyethyleneimine (molecular weight 600Da) solution, and reacted in a 60°C water bath for 2 hours. The membrane fibers were then taken out and immersed in pure water for 12 hours. The water was changed every 1 hour. The membrane fibers were then taken out and immersed in an aqueous solution containing 50% by volume of glycerol for 24 hours. The membrane fibers were taken out and dried at room temperature away from light to obtain a positively charged hollow fiber nanofiltration membrane.

[0067] Example 2

[0068] The difference between this embodiment and embodiment 1 is that in step (4), the molecular weight of polyethyleneimine is 25000Da.

[0069] Example 3

[0070] The difference between this embodiment and embodiment 1 is that in step (4), the molecular weight of polyethyleneimine is 70000Da.

[0071] Comparative Example 1

[0072] The difference between this comparative example and Example 1 is that in step (2), the mass percentage of the oligomer is 0%, and step (4) is not performed.

[0073] Comparative Example 2

[0074] The difference between this comparative example and Example 1 is that in step (2), the mass percentage of the oligomer is 3%, and step (4) is not performed.

[0075] Comparative Example 3

[0076] The difference between this comparative example and Example 1 is that in step (2), the mass percentage of the oligomer is 5%, and step (4) is not performed.

[0077] Comparative Example 4

[0078] The difference between this comparative example and Example 1 is that in step (2), the mass percentage of the oligomer is 8%, and step (4) is not performed.

[0079] Test Example 1 Characterization of Hollow Fiber Nanofiltration Membrane

[0080] The surface and cross-sectional morphology of the hollow fiber nanofiltration membranes prepared in the examples and comparative examples were observed using a field emission scanning electron microscope (FESEM, model: Quanta 400). Before observation, the hollow fiber nanofiltration membranes were dried in advance using a freeze dryer; the membrane fibers were fixed on a conductive adhesive, the sample surface was gold-sprayed, and observation was performed at an accelerating voltage of 5 kV.

[0081] Figure 1 The outer surface morphology of the hollow fiber membranes prepared in Examples 1-3 and Comparative Examples 1-4 is shown in FIG. Figure 1As shown, it can be seen from Comparative Examples 1-4 that no membrane pores can be seen in the hollow fiber membranes prepared at different oligomer addition amounts, proving that the outer layer of the spun hollow fiber membrane has a dense structure. There is no obvious change in the membrane surface after polyethyleneimine cross-linking in Example 1-3, indicating that after polyethyleneimine cross-linking, the pore structure of the membrane surface is still dense, and cross-linking does not destroy the selective layer on the surface of the membrane fiber.

[0082] Figure 2 The cross-sectional morphology of the hollow fiber membrane prepared in Comparative Examples 1-4 is shown in FIG. Figure 2 As shown in the figure, after adding oligomers, finger-like holes appeared in the outer layer of the membrane. This is attributed to the fact that the addition of oligomers caused the composition of the casting solution to change, which increased the penetration rate of the coagulation bath, thus leading to the formation of finger-like holes. At the same time, the finger-like holes did not pass through the entire outer layer section, indicating that the addition of oligomers did not affect the integrity of the outer dense selective layer.

[0083] Figure 3 The cross-sectional morphology of the hollow fiber membranes prepared in Examples 1-3 and Comparative Example 3 is shown in FIG. Figure 3 As shown, after polyethyleneimine cross-linking, the thickness of the outer selective layer of the membrane filament did not change significantly, indicating that polyethyleneimine cross-linking did not affect its overall membrane structure.

[0084] Test Example 2 Characterization experiment of surface charge of hollow fiber nanofiltration membrane

[0085] The surface charge of the hollow fiber membranes prepared in the comparative example and the example was tested using an electric solid surface analyzer (model: SurPASS 3, Anton Paar). 15 hollow fiber membrane filaments were cut to 1 cm in length and attached to a 1 cm × 2 cm sample stage at equal distances. The sample stage was placed in the test chamber, and the slit width was adjusted to 90-110 μm. A scanning test was performed in a 1 mmol / L KCl buffer solution. The pH of the solution in contact with the membrane surface was regulated by dripping acid and alkali standard solutions. The pH range of the scanning test was 3 to 10. The results are shown in Figure 4 .

[0086] Figure 4 The surface charge test results of the hollow fiber membranes prepared by Examples 1-3 and Comparative Examples 1-4. It can be seen from Comparative Examples 1-4 that with the addition of oligomers and the increase in content, the surface potential of the membrane fibers gradually decreases, and the isoelectric point gradually shifts to the left. This may be because with the increase in the content of oligomers, more uncondensed silanol and epoxy groups are introduced to the membrane surface, resulting in an increase in the electronegativity of the membrane surface. Compared with Comparative Example 3, the surface potential of Example 1-3 has been significantly improved. This shows that the epoxy groups on the membrane surface react with the rich amine groups carried by polyethyleneimine, thereby achieving an electrical reversal on the membrane fiber surface, from the negative charge of the original comparative example to a positive charge.

[0087] Test Example 3: Pure water permeation flux and salt rejection rate experiment of hollow fiber nanofiltration membrane

[0088] The pure water permeation flux and MgCl2 retention rate of the hollow fiber membranes prepared in the comparative example and the example were tested, and the specific method was as follows:

[0089] Five membrane fibers were installed into a membrane module with an effective length of 22 cm, and both ends were sealed and fixed with epoxy resin. A filtration experiment was carried out on the membrane module.

[0090] (1) Pure water flux measurement

[0091] The filtration experiment was carried out using a cross-flow filtration device, and the experimental parameters were: the temperature of the filtration experiment was 25±2°C, and the test pressure was 2 bar.

[0092] At the beginning of the test, pure water was pre-pressed at 2 bar for 1 hour to reach a stable flux. The volume of pure water passing through the nanofiltration membrane was continuously measured within a certain period of time, and the permeation flux JW (L m -2 h -1 bar -1 ), the calculation formula is:

[0093]

[0094] Where V is the permeate volume, m 3 ; A is the effective area of ​​the membrane, m 2 ; t is the sample filtration time, s; ΔP is the operating pressure of the device, bar.

[0095] (2) Determination of average molecular weight cut-off

[0096] A filtration experiment was carried out using a cross-flow filtration device to obtain the retention rate R of the hollow fiber membranes prepared in the examples and comparative examples for neutral polyethylene glycols of different molecular weights (molecular weight of 600, 1000, 2000, 4000, and 6000 Da), and the average molecular weight cutoff of the hollow fiber nanofiltration membrane was characterized.

[0097] Prepare 100mg L -1 The polyethylene glycol solution was used as the raw material solution, and the raw material solution was pre-pressed at 2 bar for 1 hour to achieve a stable flux. The concentrate and permeate were collected, and the concentrations of the two were tested using a total organic carbon analyzer (TOC). The retention rate R (%) was calculated by formula (2):

[0098]

[0099] Among them, C P and C FRepresent the TOC values ​​of the permeate and concentrate, mg / L respectively.

[0100] The retention rates corresponding to PEGs of different molecular weights were measured and a retention rate-polyethylene glycol molecular weight curve was drawn based on this. The molecular weight corresponding to the point in the curve where the retention rate was 90% was the average molecular weight cut-off (MWCO) of the membrane.

[0101] (3) Determination of salt retention rate

[0102] A filtration experiment was conducted using a cross-flow filtration device to obtain the retention rate R of the hollow fiber membranes prepared in the examples and comparative examples for MgCl2, and to characterize the selectivity of the hollow fiber membranes for cations.

[0103] Prepare 100mg L -1 MgCl2 solution was used as the raw material solution. When different raw material solutions were used for testing, the raw material solution was pre-pressed at 2 bar for 30 minutes to achieve a stable flux. The concentrate and permeate were collected, and their conductivity was tested. The salt retention rate R (%) was calculated by formula (3).

[0104]

[0105] Among them, C P and C F Represent the conductivity values ​​of the permeate and concentrate, μS / cm respectively.

[0106] The pure water permeation flux, average molecular weight cut-off and MgCl2 retention rate of the hollow fiber nanofiltration membranes prepared in the comparative examples and examples are shown in Table 1.

[0107] Table 1

[0108]

[0109]

[0110] Compared with the comparative example 1 without oligomer, the pure water flux of the comparative examples 2-4 with oligomer added was significantly improved, and the average molecular weight cut-off was increased to a certain extent. This may be because some oligomers migrated into the gel bath during the phase inversion process and played the role of pore formers. In addition, the comparative example 2 with 5% oligomer added showed a higher flux and a lower average molecular weight cut-off, which was the best condition among the comparative examples 2-4. Therefore, 5% was the best oligomer dosage, and it was used as the base membrane for the preparation of the examples 1-3.

[0111] After the membrane filaments were cross-linked with polyethyleneimine, the pure water flux and average molecular weight cutoff of the membrane filaments of Examples 1-3 were significantly reduced compared to the comparative example, indicating that the addition of polyethyleneimine made the selective layer on the outer surface of the membrane filaments more compact. This is probably because polyethyleneimine and the epoxy groups on the surface of the membrane filaments were cross-linked, which played a role in shrinking the pores. In addition, the use of polyethyleneimine with a molecular weight of 25000Da (Example 2) showed a more excellent shrinking effect, and its retention rate for MgCl2 was also significantly improved, and the pure water permeation flux was comparable to that of other examples.

[0112] Test Example 4 Characterization of γ-glycidyloxypropyltrimethoxysilane oligomer

[0113] The γ-glycidyloxypropyltrimethoxysilane oligomer prepared in step (1) of Example 1 was characterized by primary mass spectrometry using a matrix-assisted laser desorption ionization time-of-flight mass spectrometer (ultrafleXtreme, Bruker Daltonics). In addition, the oligomers prepared with reaction times of 6 h, 48 h, and 72 h were characterized to clarify the synthesis of γ-glycidyloxypropyltrimethoxysilane oligomers synthesized with different hydrolysis polymerization reaction times. Methanol was used as the test solvent, and the test product amount was 1 ml.

[0114] Figure 5 is the distribution result of oligomer molecular weight under different reaction times. Figure 5 As shown in the figure, the molecular weight of γ-glycidyloxypropyltrimethoxysilane oligomer increases with the increase of reaction time. When the reaction time is 24h, the molecular weight reaches the maximum, mainly concentrated in the range of 1000-2000. When the reaction time is increased to 48h, the molecular weight remains basically unchanged. When the reaction time is too long, reaching 72h, the oligomer obtained by the reaction undergoes reverse decomposition, which is not conducive to the preparation of γ-glycidyloxypropyltrimethoxysilane oligomer. When the reaction time is 6h, the molecular weight of the prepared oligomer is too small, and it is easy to dissolve in the subsequent film formation process, and it is impossible to construct a hollow fiber membrane with reactive surface.

[0115] The foregoing examples are merely illustrative and are used to explain some features of the method of the present invention. The appended claims are intended to require the widest possible range that can be imagined, and the embodiments presented herein are demonstrated by the applicant's actual test results. Therefore, the applicant's intention is that the appended claims are not limited by the selection of examples that illustrate the features of the present invention. Some numerical ranges used in the claims also include sub-ranges therein, and changes in these ranges should also be interpreted as being covered by the appended claims where possible.

Claims

1. A method for preparing a positively charged hollow fiber nanofiltration membrane, characterized in that: The following steps are involved: S1. The γ-glycidyl ether oxypropyl trimethoxysilane oligomer additive is mixed with a polymer, a pore-forming agent and a solvent are added to prepare a hollow fiber membrane outer layer spinning casting solution; The structural formula of the γ-glycidyloxypropyltrimethoxysilane oligomer additive is as follows: Wherein, n is 5 to 13; S2. Mixing a polymer, a pore-forming agent and a solvent to prepare a hollow fiber membrane inner layer spinning casting solution; in the steps S1 and S2, the polymer is selected from one or more of polyethersulfone, polysulfone and polyvinylidene fluoride; S3. preparing a spinning core solution; S4. Extruding the outer layer spinning casting solution, the inner layer spinning casting solution and the spinning core solution of the hollow fiber membrane through a double-layer spinneret to prepare an external pressure hollow fiber membrane; S5. The external pressure hollow fiber membrane is immersed in an amine compound solution for cross-linking modification and post-treatment to obtain the positively charged hollow fiber nanofiltration membrane.

2. The preparation method according to claim 1, characterized in that: The preparation method of the γ-glycidyloxypropyltrimethoxysilane oligomer additive is as follows: under acidic conditions, γ-glycidyloxypropyltrimethoxysilane, an alcohol solvent and pure water are mixed, heated and stirred, and the solvent is removed to obtain the γ-glycidyloxypropyltrimethoxysilane oligomer additive.

3. The preparation method according to claim 2, characterized in that: The heating and stirring time is 12 to 48 hours.

4. The preparation method according to claim 1, characterized in that: Calculated by mass percentage, the outer layer spinning casting solution of the hollow fiber membrane includes: 1-10% of γ-glycidyl ether oxypropyl trimethoxy silane oligomer additive, 24-32% of polymer, 1-10% of pore former, and the balance is solvent.

5. The preparation method according to claim 1, characterized in that: Calculated by mass percentage, the inner layer spinning casting solution of the hollow fiber membrane includes: 10-24% polymer, 10-40% pore-forming agent, and the balance is solvent.

6. The preparation method according to claim 1, characterized in that: The amine compound is selected from one or more of polyethyleneimine, polyallylamine hydrochloride, polyacrylamine, ethylenediamine, and hexamethylenediamine.

7. The preparation method according to claim 1 or 6, characterized in that: The molecular weight of the amine compound is 600-70000Da.

8. The preparation method according to claim 1, characterized in that: The solvent is selected from one or more of dimethyl sulfoxide, dimethylformamide, dimethylacetamide and N-methylpyrrolidone.

9. The positively charged hollow fiber nanofiltration membrane obtained by the method for preparing the positively charged hollow fiber nanofiltration membrane according to any one of claims 1 to 8.

10. Application of the positively charged hollow fiber nanofiltration membrane according to claim 9 in the fields of sewage treatment, wastewater treatment, seawater desalination, and drinking water treatment.

Citation Information

Patent Citations

  • Modified hollow fiber nanofiltration membrane and preparation method thereof

    CN114570213A

  • Preparation method of antibacterial double-layer hollow fibrous membrane

    CN103285740A

  • Hollow fiber positively charged membrane and preparation method thereof

    CN112973481A

  • Reactive additives in membrane preparation

    CN114080266A

  • Positively charged polymer membranes

    EP1038570A1