External wall insulation formwork for building without disassembly and processing method thereof

By applying interface agent spraying and polymer mortar beaching to the cut thermosetting boards, the problem of low tensile strength of composite insulation boards is solved, allowing for higher tensile strength and the possibility of more complex facing layers.

CN117774118BActive Publication Date: 2024-10-25NANJING TIANYUN PLASTIC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311821198.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-27
Publication Date
2024-10-25
Estimated Expiration
2043-12-27

AI Technical Summary

Technical Problem

The vertical surface tensile strength of the existing composite insulation boards is low, resulting in a single method for the facing layer, which cannot meet the requirements of some pasted facing bricks.

Method used

By spraying interface agent on the cut thermosetting board to fill the loose parts of the board surface, and using polymer mortar for beaching and extrusion molding in a wet state, the tensile strength of the thermosetting board is improved.

Benefits of technology

The vertical panel tensile strength of the composite insulation board is increased to more than 0.2MPa, which meets the needs of more complex facing layers.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a processing method for a non-disassembly insulation template for building exterior walls. After a thermosetting board is cut, an interface agent is sprayed on both sides. The interface agent penetrates into loose parts of the board surface to densely fill the loose parts and repair insufficient board surface density caused by disturbance damage of the board. When the interface agent is moistened, polymer mortar is used for beach coating. On the basis of the interface agent, the penetration and shaping of the polymer mortar are combined to improve the tensile strength of the vertical board surface of the thermosetting board, and the tensile strength can be improved to above 0.2MPa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to a non-disassembly insulation template for building exterior walls and a processing method thereof. Background Art

[0002] The existing external wall non-disassembly composite insulation formwork materials are all made of insulation core materials and general plastering mortar on the market. The thermosetting board is cut as required, conveyed to the beach area, and the general polymer mortar is mixed in the mixing tank and directly applied to the thermosetting board. It is conveyed to the press area, and then formed by the scraper, and finally cured on the curing rack. After the curing is completed, it is sent to the punching and cutting workshop for final stacking. The composite insulation board produced by this traditional process will be damaged on both sides of the board due to the disturbance of the saw blade during the cutting process, which greatly reduces the tensile strength of the composite insulation board. The tensile strength of the vertical board surface of the composite insulation board is about 0.1MPa, which leads to a single finishing layer method, which can only be used as a paint finishing layer, and cannot meet some requirements for pasting facing tiles. Summary of the invention

[0003] The purpose of the present invention is to provide a non-dismantling insulation formwork for building exterior walls and a processing method thereof in order to address the problem that the existing composite insulation board has low tensile strength on the vertical surface, resulting in a single finishing layer method. The thermosetting board is repaired after cutting, combined with polymer mortar and process control, and high-pressure composite is performed on the thermosetting board to improve the tensile strength of the vertical board surface.

[0004] According to a first aspect of the present invention, there is provided a method for processing a building exterior wall non-disassembly insulation formwork, comprising the following steps:

[0005] S1, cutting the thermosetting plate into required sizes as required, and performing dust removal treatment to obtain a first intermediate;

[0006] S2, spraying an interface agent on both sides of the first intermediate to obtain a second intermediate, and ensuring that the interface agent on the second intermediate is still in a wet state when the next process is carried out; wherein, the loose part of the board surface is filled with a closed chamber through the penetration of the interface agent;

[0007] S3, applying polymer mortar on both sides of the second intermediate within the first temperature range to obtain a third intermediate;

[0008] S4, laying a first mesh cloth on both sides of the third intermediate, then applying polymer mortar on the first mesh cloth again, and then laying a second mesh cloth on the mortar after applying the mortar, to obtain a fourth intermediate;

[0009] S5, after the fourth intermediate is extruded and formed, it is placed on a curing rack for curing, and after the curing is completed, it is cut, punched, and stacked to obtain a non-dismantling insulation template for the exterior wall of the building.

[0010] As an optional implementation, the interface agent comprises, by weight percentage, 40% to 50% acrylic emulsion, 30% to 48% water, 5% to 13% propylene glycol, 4% to 7% cellulose, and 1% to 2% leveling agent.

[0011] As an optional implementation, in step S2, the time for spraying the interface agent is controlled within 15 minutes to ensure that the interface agent on the second intermediate is still in a wet state when the next process is carried out.

[0012] As an optional embodiment, the polymer mortar includes a polymer component and a sand-lime component, and the mass ratio of the polymer component to the sand-lime component is 1:6.

[0013] As an optional embodiment, the polymer component includes, by weight, 10 to 15 parts of styrene, 10 to 15 parts of butyl acrylate, 1 to 5 parts of methacrylate, 1 to 5 parts of emulsifier, and 45 to 55 parts of deionized water.

[0014] As an optional embodiment, the sand-ash component includes, by weight, 200-300 parts of cement, 150-200 parts of sand, 50-100 parts of fly ash, 1-5 parts of cellulose, 1-5 parts of defoaming agent, and 2-4 parts of water repellent.

[0015] As an optional implementation manner, the first temperature range is 10-20°C.

[0016] As an optional implementation, in step S5, the mortar is formed when it is extruded until the overall thickness is 3 to 7 mm.

[0017] As an optional implementation, in step S5, the curing time is more than 48 hours.

[0018] According to a second aspect of the present invention, there is provided a building exterior wall non-disassembly insulation formwork processed by the aforementioned method.

[0019] Compared with the prior art, the present invention has the following significant beneficial effects:

[0020] The processing method of the non-removable insulation formwork for building exterior walls of the present invention comprises the following steps: after the thermosetting board is cut, an interface agent is sprayed on both sides, and the interface agent penetrates into the loose parts of the board surface to densely fill the loose parts, thereby repairing the insufficient board surface density caused by the disturbance damage of the board. When the interface agent is moistened, polymer mortar is used for beach coating, and on the basis of the interface agent, the penetration and shaping of the polymer mortar are combined to improve the tensile strength of the vertical board surface of the thermosetting board, and the tensile strength can be improved to above 0.2MPa. DETAILED DESCRIPTION

[0021] In order to better understand the technical content of the present invention, specific embodiments are given as follows.

[0022] The embodiments of the present disclosure are not necessarily intended to include all aspects of the invention.It should be understood that the various concepts and embodiments introduced above, as well as those described in more detail below, can be implemented in any of many ways.

[0023] In an exemplary embodiment of the present invention, a method for processing a building exterior wall non-disassembly insulation formwork is provided, comprising the following steps:

[0024] S1, cutting the thermosetting plate into required sizes as required, and performing dust removal treatment to obtain a first intermediate;

[0025] S2, spraying an interface agent on both sides of the first intermediate to obtain a second intermediate, and ensuring that the interface agent on the second intermediate is still in a wet state when the next process is carried out; wherein, the loose part of the board surface is filled with a closed chamber through the penetration of the interface agent;

[0026] S3, applying polymer mortar on both sides of the second intermediate within the first temperature range to obtain a third intermediate;

[0027] S4, laying a first mesh cloth on both sides of the third intermediate, then applying polymer mortar on the first mesh cloth again, and then laying a second mesh cloth on the mortar after applying the mortar, to obtain a fourth intermediate;

[0028] S5, after the fourth intermediate is extruded and formed, it is placed on a curing rack for curing, and after the curing is completed, it is cut, punched, and stacked to obtain a non-dismantling insulation template for the exterior wall of the building.

[0029] As an optional implementation, the interface agent comprises, by weight percentage, 40% to 50% acrylic emulsion, 30% to 48% water, 5% to 13% propylene glycol, 4% to 7% cellulose, and 1% to 2% leveling agent.

[0030] As an optional implementation, in step S2, the time for spraying the interface agent is controlled within 15 minutes to ensure that the interface agent on the second intermediate is still in a wet state when the next process is carried out.

[0031] As an optional embodiment, the polymer mortar includes a polymer component and a sand-lime component, and the mass ratio of the polymer component to the sand-lime component is 1:6.

[0032] As an optional embodiment, the polymer component includes, by weight, 10 to 15 parts of styrene, 10 to 15 parts of butyl acrylate, 1 to 5 parts of methacrylate, 1 to 5 parts of emulsifier, and 45 to 55 parts of deionized water.

[0033] As an optional embodiment, the sand-ash component includes, by weight, 200-300 parts of cement, 150-200 parts of sand, 50-100 parts of fly ash, 1-5 parts of cellulose, 1-5 parts of defoaming agent, and 2-4 parts of water repellent.

[0034] As an optional implementation manner, the first temperature range is 10-20°C.

[0035] As an optional implementation, in step S5, the mortar is formed when it is extruded until the overall thickness is 3 to 7 mm.

[0036] As an optional implementation, in step S5, the curing time is more than 48 hours.

[0037] It can be understood that the various materials in the interface agent, polymer component and sand ash component of the present invention can be directly purchased from the market.

[0038] In another exemplary embodiment of the present invention, a non-disassembly insulation formwork for building exterior walls processed by the aforementioned method is provided.

[0039] The above method and the obtained insulation template are tested in combination with specific examples.

[0040] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, etc. used in the following embodiments can be obtained from commercial sources unless otherwise specified.

[0041] Example 1

[0042] Cut the thermosetting plate into the required size (length × width × height = 1000mm × 1000mm × 65mm) as required, and carry out dust removal. Then spray the interface agent on both sides. Control the spraying process within 15 minutes to ensure that the interface agent is still in a wet state when carrying out the next process.

[0043] The thermosetting plate after spraying the interface agent is transported to the beach area via a conveyor belt, and the polymer mortar is beach-coated on both sides of the thermosetting plate at a temperature of 15°C. Then, the first mesh cloth is laid on both sides of the thermosetting plate, and then the polymer mortar is beach-coated on the first mesh cloth again. The second mesh cloth is laid on the mortar after beach coating. After laying, the mortar is extruded until the overall thickness is 5 mm to obtain a molded part.

[0044] Place the molded parts on the curing rack for curing for 60 hours. After curing, send them to the punching and cutting workshop for manual cutting and finally stacking.

[0045] The interface agent components used are as follows according to mass percentage: 50% acrylic emulsion, 35% water, 10% propylene glycol, 4% cellulose (HBR250), and 1% leveling agent Kathon LX.

[0046] The polymer component and the sand-lime component are mixed in a mass ratio of 1:6 to obtain a polymer mortar;

[0047] The polymer components used are as follows in parts by weight: 15 parts of styrene, 15 parts of butyl acrylate, 4 parts of methacrylate, 2 parts of emulsifier (sodium dodecyl sulfate), and 55 parts of deionized water.

[0048] The sand and ash components used are as follows: 300 parts of 42.5 cement, 200 parts of 70-140 mesh sand, 60 parts of fly ash, 5 parts of cellulose (75,000 viscosity), 2 parts of defoaming agent, and 3 parts of water repellent.

[0049] Comparative Example 1

[0050] Cut the thermosetting plate into the required size (length × width × height = 1000mm × 1000mm × 65mm) as required, and carry out dust removal. Then spray the interface agent on both sides. Control the spraying process within 15 minutes to ensure that the interface agent is still in a wet state when carrying out the next process.

[0051] The thermosetting plate after spraying the interface agent is transported to the beach area via a conveyor belt, and the mortar is applied on both sides of the thermosetting plate. Then, the first mesh cloth is laid on both sides of the thermosetting plate, and then the polymer mortar is applied on the first mesh cloth again. The second mesh cloth is laid on the mortar after the application. After the laying is completed, the mortar is extruded until the overall thickness is 5 mm to obtain a molded part.

[0052] Place the molded parts on the curing rack for curing for 60 hours. After curing, send them to the punching and cutting workshop for manual cutting and finally stacking.

[0053] The interface agent components used are as follows according to mass percentage: 50% acrylic emulsion, 35% water, 10% propylene glycol, 4% cellulose (HBR250), and 1% leveling agent Kathon LX.

[0054] The mortar is a mixture of sand-lime components and water in a mass ratio of 6:1;

[0055] The sand and ash components used are as follows: 300 parts of 42.5 cement, 200 parts of 70-140 mesh sand, 60 parts of fly ash, 5 parts of cellulose (75,000 viscosity), 2 parts of defoaming agent, and 3 parts of water repellent.

[0056] Comparative Example 2

[0057] The thermosetting plate is cut into the required size (length×width×height=1000mm×1000mm×65mm) as required and dust-removed.

[0058] The dust-removed thermosetting plate is transported to the beach area via a conveyor belt, and the mortar is applied on both sides of the thermosetting plate. Then, the first mesh cloth is laid on both sides of the thermosetting plate, and then the polymer mortar is applied on the first mesh cloth again. The second mesh cloth is laid on the mortar after the application. After the laying is completed, the mortar is extruded until the overall thickness is 5 mm to obtain a molded part.

[0059] Place the molded parts on the curing rack for curing for 60 hours. After curing, send them to the punching and cutting workshop for manual cutting and finally stacking.

[0060] The mortar is a mixture of sand-lime components and water in a mass ratio of 6:1;

[0061] The sand and ash components used are as follows: 300 parts of 42.5 cement, 200 parts of 70-140 mesh sand, 60 parts of fly ash, 5 parts of cellulose (75,000 viscosity), 2 parts of defoaming agent, and 3 parts of water repellent.

[0062] test

[0063] The samples of Example 1 and Comparative Example 1 were sent to Jiangsu Province Construction Engineering Quality Inspection Center to test the tensile strength perpendicular to the board surface.

[0064] Testing equipment: FM1524 microcomputer-controlled electronic universal testing machine; LS14638 digital display vernier caliper

[0065] The test results show that the tensile strength of the insulation formwork processed by the method of the present invention is 0.21 MPa in the direction perpendicular to the board surface; the tensile strength of the sample of comparative example 1 in the direction perpendicular to the board surface is 0.15 MPa, and the tensile strength of the sample of comparative example 2 in the direction perpendicular to the board surface is 0.12 MPa.

[0066] It can be seen that by adopting the method of the present invention, the tensile strength of the thermal insulation formwork in the direction perpendicular to the board surface is improved through the combination of the interface agent, the polymer mortar and the process.

[0067] Although the present invention has been disclosed as above with preferred embodiments, it is not intended to limit the present invention. A person with ordinary knowledge in the technical field to which the present invention belongs may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be determined by the definition of the claims.

Claims

1. A method for processing a building exterior wall non-disassembly insulation formwork, characterized in that: The following steps are involved: S1, cutting the thermosetting plate into required sizes as required, and performing dust removal treatment to obtain a first intermediate; S2, spraying an interface agent on both sides of the first intermediate, the time of spraying the interface agent is controlled within 15 minutes to ensure that the interface agent on the second intermediate is still in a wet state when the next step is carried out, to obtain a second intermediate; Among them, the loose parts of the board surface are densely filled through the penetration of the interface agent; The interface agent comprises, by weight percentage, 40% to 50% acrylic emulsion, 30% to 48% water, 5% to 13% propylene glycol, 4% to 7% cellulose, and 1% to 2% leveling agent; S3, applying polymer mortar on both sides of the second intermediate at a temperature of 10-20° C. to obtain a third intermediate; S4, laying a first mesh cloth on both sides of the third intermediate, then applying polymer mortar on the first mesh cloth again, and then laying a second mesh cloth on the mortar after applying the mortar, to obtain a fourth intermediate; The polymer mortar comprises a polymer component and a sand-ash component. The polymer component comprises, by weight, 10 to 15 parts of styrene, 10 to 15 parts of butyl acrylate, 1 to 5 parts of methacrylate, 1 to 5 parts of emulsifier, and 45 to 55 parts of deionized water. S5. After the fourth intermediate is extruded and formed, it is placed on a curing rack for curing. After the curing is completed, it is cut, punched, and stacked to obtain a non-disassembly insulation formwork for building exterior walls; wherein the tensile strength of the insulation formwork is increased to above 0.2Mpa.

2. The method for processing the building exterior wall non-disassembly insulation formwork according to claim 1, characterized in that: The mass ratio of the polymer component to the sand-ash component is 1:

6.

3. The method for processing the building exterior wall non-disassembly insulation formwork according to claim 1, characterized in that: The sand-ash components include, by weight, 200-300 parts of cement, 150-200 parts of sand, 50-100 parts of fly ash, 1-5 parts of cellulose, 1-5 parts of defoaming agent, and 2-4 parts of water repellent.

4. The method for processing the building exterior wall non-disassembly insulation formwork according to claim 1, characterized in that: In the step S5, the mortar is formed by extruding until the overall thickness is 3-7 mm.

5. The method for processing the building exterior wall non-disassembly insulation formwork according to claim 1, characterized in that: In step S5, the curing time is more than 48 hours.

6. A non-disassembly insulation formwork for building exterior walls processed by the method described in any one of claims 1 to 5.