Preparation method of highly elastic hydrophobic radiation-cured wood lacquer skin-feel coating

By directly coating the surface of the wood with hyperbranched nanocellulose hydrogel and radiation light curing coating, the use of the porous structure of the wood to form a skin-like wrinkle texture, solving the problem that the natural skin touch cannot be achieved in the prior art, and achieving the High efficiency coating with high elasticity and durability.

CN117801653BActive Publication Date: 2024-11-22INST OF WOOD INDUDTRY CHINESE ACAD OF FORESTRY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311865139.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-29
Publication Date
2024-11-22
Estimated Expiration
2043-12-29

AI Technical Summary

Technical Problem

Existing wood coating technology is difficult to effectively utilize the porous structure and nanocellulose of wood, and it is impossible to achieve a decorative effect similar to the touch of natural skin.

Method used

Hyperbranched nanocellulose hydrogel combined with radiation photocuring coating, and through the synthesis, modification and grafting of hyperbranched polymers, a highly elastic hydrophobic radiation cured wood paint with micron and nano-scale folds is formed. The layer, using physical filling of wood cells and cellulose fibers to form a skin-like wrinkle texture.

Benefits of technology

It realizes the skin tactile performance of the wood surface, improves the physical and mechanical properties and durability of the coating, and has excellent characteristics such as low gloss, hydrophobicity and self-cleaning.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117801653B_ABST
    Figure CN117801653B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a highly elastic and hydrophobic radiation-cured wood lacquer skin-feel coating, comprising the following steps: S1. synthesis of a hyperbranched polymer; S2. modification and grafting of a nanocellulose hydrogel by a hyperbranched polymer; S3. preparation of a modified radiation-cured water-based skin-feel coating; S4. roller coating of a highly elastic and hydrophobic radiation-cured wood lacquer skin-feel coating; the invention is based on directly coating a radiation-cured coating with a hyperbranched nanocellulose hydrogel added thereto on a porous structure of wood to construct micron-scale and nanometer-scale wrinkles, thereby achieving skin-tactile properties of the coating on the surface of the wood; the hyperbranched nanocellulose hydrogel can be better dispersed in the coating; the physical and mechanical properties and durability of the coating are improved by reacting the ‑NH2 group in the hyperbranched nanocellulose hydrogel with the ‑NCO group of a polyurethane acrylate resin in the radiation-cured coating; in addition, the coating also has excellent properties such as low gloss, hydrophobicity and self-cleaning properties, and good elasticity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wood coatings, and in particular to a method for preparing a highly elastic and hydrophobic radiation-cured wood lacquer skin-feel coating. Background Art

[0002] With the wide application of wood-based decorative materials in various fields, wood coatings not only need to meet the basic coating performance, but also people's demand for the subjective feeling of decorative materials for different application occasions is also increasing. Decorative materials that can bring a comfortable touch to people are more and more popular, and skin-feel coatings with skin-feel performance are produced. Radiation-cured coatings based on acrylates can be used to prepare wood coatings with self-wrinkling surface skin-feel effects by combining curing with excimer lamps and ultraviolet light. At present, the market generally first applies adhesion primer, putty or sanding primer to avoid substrate defects and provide a smooth surface, and then applies skin-feel topcoat and cures to obtain a self-wrinkling skin-feel effect.

[0003] Wood itself is a porous material with a wrinkled structure from nanometer to macroscale. For example, the diameter of wood cells is between 10 μm and 400 μm, the diameter of the pores on the cell wall is between 10 nm and 8 μm, and the gap between the cell wall microfibrils is between 2 nm and 4.5 nm. However, in the usual finishing process, the pores of the wood itself are not utilized. Therefore, providing a method to achieve a surface decoration effect similar to the touch of natural skin by combining the multi-scale structure of natural wood and the skin-feel coating enhanced by nanocellulose is a problem that needs to be solved urgently. Summary of the invention

[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing a highly elastic and hydrophobic radiation-cured wood lacquer skin-feel coating. The present invention is based on directly coating the surface of the porous structure of the wood with a radiation-cured coating with added hyperbranched nanocellulose hydrogel to construct micron- and nanometer-scale wrinkles, thereby achieving the skin-tactile properties of the coating on the wood surface. The hyperbranched nanocellulose hydrogel can be better dispersed in the coating, and the physical and mechanical properties and durability of the coating are improved through the reaction of the -NH2 group in the hyperbranched nanocellulose hydrogel and the -NCO group of the polyurethane acrylate resin in the radiation-cured coating. In addition, the coating also has excellent properties such as low gloss, hydrophobicity and self-cleaning, and good elasticity.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A method for preparing a highly elastic and hydrophobic radiation-cured wood lacquer skin-feel coating comprises the following steps:

[0007] S1. Synthesis of hyperbranched polymers:

[0008] Diethylenetriamine is placed in a three-necked flask and cooled with an ice-water bath. Under nitrogen protection, methyl acrylate-methanol solution is dripped into the flask at a stirring speed of 100-150 r / min. After reacting at 23-27°C for 3-5 hours, the methanol solvent is removed by a rotary evaporator. The flask is then transferred to an oil bath and reacted at 148-152°C for 4-6 hours to obtain a hyperbranched polymer containing an amino group at the end;

[0009] S2. Modification and grafting of nanocellulose hydrogels with hyperbranched polymers

[0010] S201. Modification of nanocellulose hydrogel: After adjusting the pH value of the nanocellulose hydrogel to 5.0 using 0.1-0.3 mol / L hydrochloric acid solution, 5-8 mmol / L NaIO4 was added into the flask, and the reaction was carried out at 38-50 °C and 800-1200 r / min in the dark for 6-8 hours to obtain the modified nanocellulose hydrogel, which was recorded as D-CNF.

[0011] S202. The modified nanocellulose hydrogel is adjusted to a solution with a solid content of 2.0% with distilled water;

[0012] S203. Grafting of hyperbranched polymer: Grafting the hyperbranched polymer into the solution of modified nanocellulose hydrogel in S202, stirring at a speed of 300-500 r / min in an ice-water bath for 2-4 hours, to obtain a hyperbranched nanocellulose hydrogel, denoted as HB-CNF;

[0013] S204. The hyperbranched nanocellulose hydrogel was adjusted to a solution having a solid content of 2.0% with distilled water;

[0014] S3. Preparation of modified radiation-curable water-based skin-feel coating: adding a 2.0% hyperbranched nanocellulose hydrogel solution to a radiation-curable water-based skin-feel coating in an amount of 2-8% by mass of the coating, and dispersing at a stirring speed of 2000-4000 r / min for 30-40 min to obtain a modified radiation-curable water-based skin-feel coating;

[0015] S4. Roller coating of highly elastic hydrophobic radiation-cured wood lacquer skin-feel coating:

[0016] S401. Roller-coat the coating in step S3 evenly on the sanded plywood, with a wet coating thickness of 30-50 μm; S402. Dry the plywood treated in S401 for 1-2 min with an infrared dryer at a dehydration power of 2-4 kW; then,

[0017] Pre-curing with 254 nm excimer lamp, curing energy is 10-15 mJ / cm 2 Finally, a mercury lamp is used for full dry curing, the UV radiation intensity is 250-350 mJ / cm2, and the radiation time is 3-5s, so as to form a highly elastic and hydrophobic radiation-cured wood paint skin-feel coating on the plywood.

[0018] Preferably, in S1, the mass ratio of diethylenetriamine to methyl acrylate-methanol solution is 8-10:4-5:1.

[0019] Preferably, in S202, the aldehyde group of the modified nanocellulose hydrogel is 1.84 mmol / g.

[0020] Preferably, in S203, the mass ratio of the modified nanocellulose hydrogel to the hyperbranched polymer is 5-15:1.

[0021] Preferably, in S1, the amount of methanol added to the methyl acrylate-methanol solution is sufficient to completely dissolve the methyl acrylate.

[0022] Preferably, in S203, the preparation route and structure of the hyperbranched nanocellulose hydrogel are as follows:

[0023] .

[0024] Preferably, in S3, the radiation light-curable water-based coating comprises, by mass percentage:

[0025] Ammonium carboxylate water-emulsified hexafunctional polyurethane acrylate resin 10-30%, hexafunctional fluorosilicone resin 10-20%, trifunctional polyurethane resin 15-30%, acyl acid monomer 10-20%, photoinitiator 0.2-1.0%, leveling agent 0.1-0.5%, defoaming agent 0.1-0.5%, matting powder 0.1-0.5% and water 20-40%.

[0026] Preferably, the acyl acid monomer is hydroxyethyl methacrylate monomer.

[0027] Preferably, the photoinitiator is one or more of acylphosphine oxides, α-hydroxyketone derivatives, and thioxanthone;

[0028] The leveling agent is a polyether-modified silicone leveling agent, further limited to one or more of BYK-373, BYK-333 or TEGO-410.

[0029] Preferably, the defoaming agent is polysiloxane-polyether copolymer TEGO-810;

[0030] The matting powder is a meteoric silica matting powder; further defined as E-1011.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] 1. The present invention is based on the direct coating of the radiation photocuring coating with HB-CNF added on the surface of the porous structure of wood to construct wrinkles including micron-scale and nano-scale, and realize the skin-tactile performance of the coating on the wood surface. The principle is mainly to physically fill the wood cells with the coating to produce micro-wrinkles with a width of about 12-15 μm and a height of about 12-15 μm. In the nanoscale range, there are some protrusions formed by the filling of CNF fibers with HB-CNF fibers in the pores, the protrusions generated by the HB-CNF structure itself, and the protrusions at 50-100 nm formed by the reaction of HB-CNF and the coating. These factors form the internal and external micro-nanoscale wrinkled textures similar to skin;

[0033] 2. HB-CNF can be better dispersed in the coating, and the physical and mechanical properties and durability of the coating are improved through the reaction of the –NH2 group in HB-CNF and the –NCO group of the polyurethane acrylate resin in the radiation photocuring coating; in addition, the coating has excellent properties such as low gloss, hydrophobicity and self-cleaning, and good elasticity. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 The present invention is a process flow chart for preparing the highly elastic and hydrophobic radiation-cured wood lacquer skin-feel coating;

[0035] Figure 2 The process flow chart of modification and grafting of the hyperbranched polymer to nanocellulose hydrogel of the present invention;

[0036] Figure 3 The process flow chart of roller coating of the highly elastic hydrophobic radiation-cured wood lacquer skin-feel coating of the present invention;

[0037] Figure 4 This is a scanning electron microscope image of the highly elastic hydrophobic radiation-cured wood lacquer skin-feel coating of the present invention;

[0038] Figure 5 This is a transmission electron microscope image of the highly elastic hydrophobic radiation-cured wood lacquer skin-feel coating of the present invention. DETAILED DESCRIPTION

[0039] The present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] See also Figure 1-5, the present invention provides a technical solution:

[0041] Embodiment 1:

[0042] A method for preparing a highly elastic and hydrophobic radiation-cured wood lacquer skin-feel coating:

[0043] S1. Synthesis of Hyperbranched Polymers:

[0044] 400 g of diethylenetriamine was placed in a three-necked flask and cooled with an ice-water bath. Under nitrogen protection, 250 g of methyl acrylate-methanol solution was dripped into the flask at a stirring speed of 100 r / min. After reacting at 23 ° C for 4 hours, the methanol solvent was removed by a rotary evaporator. The flask was then transferred to an oil bath and reacted at 148 ° C for 4 hours to obtain a hyperbranched polymer containing amino groups at the end.

[0045] S2. Modification and grafting of CNF with hyperbranched polymers:

[0046] S201. Modification of nanocellulose hydrogel: After adjusting the pH value of CNF hydrogel to 5.0 using 0.1 mol / L hydrochloric acid solution, 6.0 mmol / L NaIO4 was added into the flask and reacted at 38°C and stirring speed of 1000 r / min for 6 h in the dark to obtain modified nanocellulose hydrogel, which was recorded as D-CNF;

[0047] S202. The modified nanocellulose hydrogel is adjusted to a solution with a solid content of 2.0% with distilled water;

[0048] S203. Grafting of hyperbranched polymer: The hyperbranched polymer prepared in S1 was grafted onto D-CNF, with the mass ratio of D-CNF to hyperbranched polymer being 10:1. After reacting for 4 h in an ice-water bath bottle at a stirring speed of 400 r / min, a hyperbranched nanocellulose hydrogel was obtained, which was recorded as HB-CNF.

[0049] S204. The hyperbranched nanocellulose hydrogel was adjusted to a solution having a solid content of 2.0% with distilled water;

[0050] S3. Preparation of modified radiation-curable water-based skin-feel coating: HB-CNF with a solid content of 2.0% was added to the radiation-curable water-based skin-feel coating in an amount of 2% of the coating mass, and the mixture was dispersed at a stirring speed of 3000 r / min for 30 min to obtain a modified radiation-curable water-based skin-feel coating;

[0051] S4. Roller coating of highly elastic hydrophobic radiation-cured wood lacquer skin-feel coating:

[0052] S401. The modified radiation-cured water-based skin-feel coating in which HB-CNF was added was uniformly coated on the sanded plywood by roller coating, and the roller-coated wet coating thickness was 40 μm;

[0053] S402. The plywood treated with S401 was dried in an infrared dryer for 1 min with a dehydration efficiency of 3 kW, and then pre-cured with a 254 nm excimer lamp with a curing energy of 15 mJ / cm 2 , curing time 3s, and finally, full dry curing with a mercury lamp, the UV radiation intensity is 350 mJ / cm 2 , the irradiation time is 3 s, thereby forming a highly elastic and hydrophobic radiation-cured wood paint skin-feel coating on the plywood.

[0054] Among them, the infrared dryer model is PRT-G4, produced by Guangdong Hanqiu Intelligent Equipment Co., Ltd.;

[0055] The excimer lamp model is PRT-F3, produced by Guangdong Hanqiu Intelligent Equipment Co., Ltd.;

[0056] The mercury lamp is model PRT-G2, produced by Guangdong Hanqiu Intelligent Equipment Co., Ltd.

[0057] The radiation light-cured water-based skin-feel coating formula includes the following components by mass percentage:

[0058]

[0059] The acyl acid monomer is hydroxyethyl methacrylate monomer;

[0060] The photoinitiator is thioxanthone;

[0061] The leveling agent is BYK-373;

[0062] The defoamer is polysiloxane-polyether copolymer TEGO-810;

[0063] The matting powder is E-1011.

[0064] Example 2

[0065] A method for preparing a highly elastic and hydrophobic radiation-cured wood lacquer skin-feel coating:

[0066] S1. Synthesis of Hyperbranched Polymers:

[0067] 400 g of diethylenetriamine was placed in a three-necked flask and cooled with an ice-water bath. Under nitrogen protection, 250 g of methyl acrylate-methanol solution was dripped into the flask at a stirring speed of 100 r / min. After reacting at 27 ° C for 4 hours, the methanol solvent was removed by a rotary evaporator. The flask was then transferred to an oil bath and reacted at 152 ° C for 4 hours to obtain a hyperbranched polymer containing amino groups at the end.

[0068] S2. Modification and grafting of CNF with hyperbranched polymers:

[0069] S201. Modification of nanocellulose hydrogel: After adjusting the pH value of CNF hydrogel to 5.0 using 0.1 mol / L hydrochloric acid solution, 6.0 mmol / L NaIO4 was added into the flask and reacted at 42°C and stirring speed of 1000 r / min for 6 h in the dark to obtain modified nanocellulose hydrogel, which was recorded as D-CNF.

[0070] S202. The modified nanocellulose hydrogel is adjusted to a solution with a solid content of 2.0% with distilled water;

[0071] S203. Grafting of hyperbranched polymer: The hyperbranched polymer prepared in S1 was grafted onto D-CNF, with the mass ratio of D-CNF to hyperbranched polymer being 10:1. After reacting for 4 h in an ice-water bath bottle at a stirring speed of 400 r / min, a hyperbranched nanocellulose hydrogel was obtained, which was recorded as HB-CNF.

[0072] S204. The hyperbranched nanocellulose hydrogel was adjusted to a solution having a solid content of 2.0% with distilled water;

[0073] S3. Preparation of modified radiation-curable water-based skin-feel coating: HB-CNF with a solid content of 2.0% was added to the radiation-curable water-based skin-feel coating in an amount of 5% by mass of the coating, and the mixture was dispersed at a stirring speed of 3000 r / min for 30 min to obtain a modified radiation-curable water-based skin-feel coating;

[0074] S4. Roller coating of highly elastic hydrophobic radiation-cured wood lacquer skin-feel coating:

[0075] S401. The modified radiation-cured water-based skin-feel coating in which HB-CNF was added was uniformly coated on the sanded plywood by roller coating, and the roller-coated wet coating thickness was 40 μm;

[0076] S402. The plywood treated with S401 was dried in an infrared dryer for 1 min with a dehydration efficiency of 3 kW, and then pre-cured with a 254 nm excimer lamp with a curing energy of 15 mJ / cm 2, curing time 3s, and finally, full dry curing with a mercury lamp, the UV radiation intensity is 350 mJ / cm 2 , the irradiation time is 3 s, thereby forming a highly elastic and hydrophobic radiation-cured wood paint skin-feel coating on the plywood.

[0077] Among them, the infrared dryer model is PRT-G4, produced by Guangdong Hanqiu Intelligent Equipment Co., Ltd.;

[0078] The excimer lamp model is PRT-F3, produced by Guangdong Hanqiu Intelligent Equipment Co., Ltd.;

[0079] The mercury lamp is model PRT-G2, produced by Guangdong Hanqiu Intelligent Equipment Co., Ltd.

[0080] The radiation light-cured water-based skin-feel coating formula includes the following components by mass percentage:

[0081]

[0082] The acyl acid monomer is hydroxyethyl methacrylate monomer;

[0083] The photoinitiator is thioxanthone;

[0084] The leveling agent is BYK-333;

[0085] The defoamer is polysiloxane-polyether copolymer TEGO-810;

[0086] The matting powder is E-1011.

[0087] Example 3

[0088] A method for preparing a highly elastic and hydrophobic radiation-cured wood lacquer skin-feel coating:

[0089] S1. Synthesis of Hyperbranched Polymers:

[0090] 800 g of diethylenetriamine was placed in a three-necked flask and cooled with an ice-water bath. Under nitrogen protection, 250 g of methyl acrylate-methanol solution was dripped into the flask at a stirring speed of 100 r / min. After reacting at 25°C for 4 hours, the methanol solvent was removed by a rotary evaporator. The flask was then transferred to an oil bath and reacted at 150°C for 4 hours to obtain a hyperbranched polymer containing amino groups at the end.

[0091] S2. Modification and grafting of CNF with hyperbranched polymers:

[0092] S201. Modification of nanocellulose hydrogel: After adjusting the pH value of CNF hydrogel to 5.0 using 0.1 mol / L hydrochloric acid solution, 6.0 mmol / L NaIO4 was added into the flask and reacted at 40°C and stirring speed of 1000 r / min for 6 h in the dark to obtain modified nanocellulose hydrogel, which was recorded as D-CNF;

[0093] S202. The modified nanocellulose hydrogel is adjusted to a solution with a solid content of 2.0% with distilled water;

[0094] S203. Grafting of hyperbranched polymer: The hyperbranched polymer prepared in S1 was grafted onto D-CNF, with the mass ratio of D-CNF to hyperbranched polymer being 10:1. After reacting for 4 h in an ice-water bath bottle at a stirring speed of 400 r / min, a hyperbranched nanocellulose hydrogel was obtained, which was recorded as HB-CNF.

[0095] S204. The hyperbranched nanocellulose hydrogel was adjusted to a solution having a solid content of 2.0% with distilled water;

[0096] S3. Preparation of modified radiation-curable water-based skin-feel coating: HB-CNF with a solid content of 2.0% was added to the radiation-curable water-based skin-feel coating in an amount of 8% by mass of the coating, and the mixture was dispersed at a stirring speed of 3000 r / min for 30 min to obtain a modified radiation-curable water-based skin-feel coating;

[0097] S4. Roller coating of highly elastic hydrophobic radiation-cured wood lacquer skin-feel coating:

[0098] S401. The modified radiation-cured water-based skin-feel coating in which HB-CNF was added was uniformly coated on the sanded plywood by roller coating, and the roller-coated wet coating thickness was 40 μm;

[0099] S402. The plywood treated with S401 was dried in an infrared dryer for 1 min with a dehydration efficiency of 3 kW, and then pre-cured with a 254 nm excimer lamp with a curing energy of 15 mJ / cm 2 , curing time 3s, and finally, full dry curing with a mercury lamp, the UV radiation intensity is 350 mJ / cm 2 , the irradiation time is 3 s, thereby forming a highly elastic and hydrophobic radiation-cured wood paint skin-feel coating on the plywood.

[0100] Among them, the infrared dryer model is PRT-G4, produced by Guangdong Hanqiu Intelligent Equipment Co., Ltd.;

[0101] The excimer lamp model is PRT-F3, produced by Guangdong Hanqiu Intelligent Equipment Co., Ltd.;

[0102] The mercury lamp is model PRT-G2, produced by Guangdong Hanqiu Intelligent Equipment Co., Ltd.

[0103] The radiation light-cured water-based skin-feel coating formula includes the following components by mass percentage:

[0104]

[0105] The acyl acid monomer is hydroxyethyl methacrylate monomer;

[0106] The photoinitiator is thioxanthone;

[0107] The leveling agent is BYK-373;

[0108] The defoamer is polysiloxane-polyether copolymer TEGO-810;

[0109] The matting powder is E-1011.

[0110] Comparative Example

[0111] Comparative Example 1: Comparative Example 1 differs from Example 1 only in that, in Comparative Example 1, steps S1, S2, and S3 originally existing in Example 1 are omitted, thereby omitting the steps of “synthesis of hyperbranched polymer”, “modification and grafting of nanocellulose hydrogel with hyperbranched polymer”, and “preparation of modified radiation-cured water-based skin-feel coating” in turn. In Comparative Example 1, only the radiation-cured water-based skin-feel coating is used to carry out the roller coating operation described in step S4, and the remaining steps are exactly the same in Comparative Example 1 and Example 1.

[0112] Performance Testing:

[0113] Characterization and testing of surface performance of decorative panels:

[0114] (1) Static contact angle test: A 4 μL drop of distilled water was dripped at 25 ± 2 °C using a contact angle meter. The sliding contact angle was determined by tilting the sample stage until the droplet began to move and roll off the sample surface.

[0115] (2) The morphology of the sample was observed using a scanning electron microscope at an accelerating voltage of 15 kV. The fine morphology of the particles was observed using a transmission electron microscope. Figure 4 and Figure 5 ;

[0116] (3) The coating adhesion and the wear resistance of the paint film were tested according to GB / T 37005-2018 Paint-finished Artificial Board. The load weight for the wear resistance test was 500 g, 180-grit sandpaper was used, and the abrasion was 100 revolutions;

[0117] (4) Compressive elastic properties were measured using a universal mechanical testing machine in compression mode. After measuring the initial thickness (t0), a stainless steel cylindrical indenter with a cross-sectional diameter of 28.7 mm was applied to the center of the coating surface at an extrusion speed of 1 mm / min. After pressing 2.82 mm and holding for 30 min, the load was unloaded and the compressed sample was placed at 25 ± 2℃ and 65% RH for 24 h. The thickness (t1) was measured again.

[0118] According to formula (1), the compression elastic performance was evaluated by testing the thickness rebound rate. This was repeated for 5 groups of samples. The test results are shown in Table 1.

[0119] (1)

[0120] Table 1 Surface properties of veneer panels

[0121]

[0122] Figure 4 It can be seen that when the HB-CNF addition amount in Example 2 is 5%, the coating water contact angle is about 123°, which has better surface hydrophobicity compared with the other three, and the sliding of HB-CNF is the smallest, with an average value of 2.4°, and it has better self-cleaning performance. Figure 5 It can be seen that the SEM image shows that the coating covers the wood surface, forming wrinkles of different heights. However, in the pits and ducts, some wrinkles disappear (see arrows). For some pits with a diameter of about 20 μm, there are some CNF fibers (see the enlarged rectangular image) filled with HB-CNF fibers to form bulges, bulges generated by the HB-CNF structure itself, and bulges at 50~100 nm formed by the reaction of HB-CNF and coating, forming a skin-like wrinkled texture inside and outside. As shown in Table 1, the embodiment of the coating with HB-CNF added has enhanced hardness, enhanced coating elasticity, and decreased gloss in the test. In summary, based on the direct coating of the radiation light-cured coating with HB-CNF added on the porous structure of wood, micron- and nano-scale wrinkles are constructed, and the skin-tactile properties of the coating on the wood surface are achieved, and the surface properties are still good in the case of thin coating.

[0123] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a highly elastic and hydrophobic radiation-cured wood lacquer skin-feel coating, characterized in that: The following steps are involved: S1. Synthesis of hyperbranched polymers: Diethylenetriamine is placed in a three-necked flask and cooled with an ice-water bath. Under nitrogen protection, methyl acrylate-methanol solution is dripped into the flask at a stirring speed of 100-150 r / min. After reacting at 23-27°C for 3-5 hours, the methanol solvent is removed by a rotary evaporator. The flask is then transferred to an oil bath and reacted at 148-152°C for 4-6 hours to obtain a hyperbranched polymer containing an amino group at the end; S2. Modification and grafting of nanocellulose hydrogels with hyperbranched polymers: S201. Modification of nanocellulose hydrogel: After adjusting the pH value of the nanocellulose hydrogel to 5.0 using 0.1-0.3 mol / L hydrochloric acid solution, 5-8 mmol / L NaIO4 was added into the flask, and the reaction was carried out at 38-50 °C and 800-1200 r / min in the dark for 6-8 hours to obtain the modified nanocellulose hydrogel, which was recorded as D-CNF. S202. The modified nanocellulose hydrogel is adjusted to a solution with a solid content of 2.0% with distilled water; S203. Grafting of hyperbranched polymer: Grafting the hyperbranched polymer into the solution of modified nanocellulose hydrogel in S202, stirring at a speed of 300-500 r / min in an ice-water bath for 2-4 hours, to obtain a hyperbranched nanocellulose hydrogel, denoted as HB-CNF; S204. The hyperbranched nanocellulose hydrogel was adjusted to a solution having a solid content of 2.0% with distilled water; S3. Preparation of modified radiation-curable water-based skin-feel coating: adding a hyperbranched nanocellulose hydrogel solution with a solid content of 2.0% to a radiation-curable water-based skin-feel coating in an amount of 2-8% by mass of the coating, and dispersing at a stirring speed of 2000-4000 r / min for 30-40 min to obtain a modified radiation-curable water-based skin-feel coating; S4. Roller coating of highly elastic hydrophobic radiation-cured wood lacquer skin-feel coating: S401. The coating in step S3 is uniformly applied by roller on the sanded plywood, and the wet coating thickness of the roller is 30-50 μm; S402. The plywood treated by S401 is dried for 1-2 min with an infrared dryer, and the dehydration power is 2-4 kW; then, Pre-curing with 254 nm excimer lamp, curing energy is 10-15 mJ / cm 2 Finally, a mercury lamp is used for full dry curing, and the UV radiation intensity is 250-350 mJ / cm 2 , the radiation time is 3-5s, thereby forming a highly elastic and hydrophobic radiation-cured wood paint skin-feel coating on the plywood; In S1, the mass ratio of diethylenetriamine to methyl acrylate-methanol solution is 8-10:4-5:1; In S203, the mass ratio of the modified nanocellulose hydrogel to the hyperbranched polymer is 5-15:1; In S3, the radiation light-curable water-based skin-feel coating comprises, by mass percentage: Ammonium carboxylate water-emulsified hexafunctional polyurethane acrylate resin 10-30%, hexafunctional fluorosilicone resin 10-20%, trifunctional polyurethane resin 15-30%, hydroxyethyl methacrylate monomer 10-20%, photoinitiator 0.2-1.0%, leveling agent 0.1-0.5%, defoaming agent 0.1-0.5%, matting powder 0.1-0.5% and water 20-40%.

2. The method for preparing a highly elastic and hydrophobic radiation-cured wood lacquer skin-feel coating according to claim 1, characterized in that: In S202, the aldehyde group of the modified nanocellulose hydrogel is 1.84 mmol / g.

3. The method for preparing a highly elastic and hydrophobic radiation-cured wood lacquer skin-feel coating according to claim 1, characterized in that: In S1, the amount of methanol added to the methyl acrylate-methanol solution is based on the amount of methanol that is just enough to completely dissolve the methyl acrylate.

4. The method for preparing a highly elastic and hydrophobic radiation-cured wood lacquer skin-feel coating according to claim 1, characterized in that: S203 In the present invention, the preparation route and structure of the hyperbranched nanocellulose hydrogel are as follows: 。 5. The method for preparing a highly elastic and hydrophobic radiation-cured wood lacquer skin-feel coating according to claim 1, characterized in that: The photoinitiator is one or more of acylphosphine oxides, α-hydroxyketone derivatives, and thioxanthone; The leveling agent is a polyether-modified silicone leveling agent, which is one or more of BYK-373, BYK-333 or TEGO-410.

6. The method for preparing a highly elastic and hydrophobic radiation-cured wood lacquer skin-feel coating according to claim 1, characterized in that: The defoamer is polysiloxane-polyether copolymer TEGO-810; The matting powder is meteorological silica matting powder; it is E-1011.