Steel for 1500MPa battery pack for new energy vehicles and preparation method thereof
By reasonably proportioning C, Si, Al, Mn, Cr, Mo, B, Ti, P and S elements in steel plates for new energy vehicles, forming specific microstructures and using fine process treatment, the existing steel plates are solved. The problems of insufficient strength attenuation and hole reaming performance at high temperatures have achieved a comprehensive effect of high yield strength and good hole reaming performance.
Patent Information
- Application Number
- CN202310476371.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-04-28
AI Technical Summary
The existing 1500MPa grade steel plates used in new energy vehicles have severe strength attenuation at high temperatures, making it difficult to meet the safety and strength requirements of the battery pack. At the same time, their hole reaming performance and surface quality are insufficient, which limits their industrial applications.
Using the reasonable proportions of steel materials with specific chemical compositions, including C, Si, Al, Mn, Cr, Mo, B, Ti, P and S, to form the critical area ferrite, tempered martensite and carbide microscope The structure controls the microstructure and surface quality of the steel plate through fine smelting, hot rolling, pickling, cold rolling and degalvanizing processes, and improves its tensile strength, yield strength and porosity reaming.
The tensile strength of 1500MPa or above, the yield strength of 1200 to 1350MPa and the elongation of ≥8%. At the same time, the yield attenuation at isothermal at 400℃ and 800℃ is less than 300MPa and 600MPa, ensuring the high temperature stability and expansion of the steel plate. Hole performance, suitable for flange forming parts of battery packs.
Smart Images

Figure BDA0004205640580000071 
Figure BDA0004205640580000072 
Figure BDA0004205640580000081
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of metal materials, and in particular relates to a 1500MPa cold-rolled alloyed hot-dip galvanized battery pack steel for new energy vehicles and a preparation method thereof. Background Art
[0002] New energy vehicles are the development trend of the automobile industry in response to the global "dual carbon" strategy. Replacing traditional fuel vehicles effectively solves the problems of energy consumption and carbon emissions. Therefore, in recent years, new energy vehicles have also become the focus of research and development of the automobile industry and related companies around it, among which battery pack materials are the focus of research and development of steel companies. The battery pack is composed of an upper cover, a crossbeam, a frame, and a lower plate. The functions of the crossbeam and frame are to ensure the safety of the battery pack, ensure the installation strength of the module, effectively resist side impact, and ensure the safety of the internal battery module. In this way, high-strength steel or ultra-high-strength steel is required for the crossbeam and frame. At present, the steel for the crossbeam and frame is mainly based on traditional high-strength steel, such as high-strength dual-phase steel, complex phase steel, martensitic steel, quenching and partitioning steel, etc. For example, MS1500 is mainly used for the crossbeam of the battery pack, but the plasticity of 1500MPa grade martensitic steel is only about 3%, and it is difficult to meet the deformation requirements even as a beam.
[0003] The publication number is CN108018484B. "Cold-rolled high-strength steel with tensile strength of more than 1500MPa and excellent formability and its manufacturing method" adopts the process idea of quenching and partitioning, and uses martensite + austenite structure to produce cold-rolled annealed steel plates with tensile strength of more than 1500MPa and elongation greater than 12%. This product does not indicate whether its hole expansion performance is good or not.
[0004] The yield strength in the embodiment shows that most of the products have the characteristics of low yield and high tensile strength, and it is difficult to ensure high hole expansion performance. Therefore, it is not suitable for flanging forming parts.
[0005] Publication number: CN112063931A, "A low-carbon medium-manganese high-residue austenite high-toughness steel and its heat treatment method" discloses a high-toughness steel alloy composition of C: 0.10% to 0.25%, Mn: 4.0% to 8.0%, Al: 1.0% to 2.5%, and the balance is Fe and inevitable inclusions. The steel plate relies on the TRIP effect provided by a large amount of austenite during the deformation process to achieve the strengthening of work hardening, thereby obtaining a 1500MPa grade steel plate. However, it is worth noting that the steel plate adds a large amount of Mn (greater than 4%) and Al (greater than 1%) elements, which seriously increases the smelting difficulty of the product. It is only suitable for laboratory research and does not have industrial prospects under current conditions; at the same time, there is an obvious Luders band in the tensile curve, which seriously affects the surface quality of the steel plate and is not conducive to stamping applications. Summary of the invention
[0006] The purpose of the present invention is to overcome the above-mentioned problems and shortcomings and to provide a 1500MPa steel for battery packs for new energy vehicles and a preparation method thereof, which can solve the problem of strength attenuation of steel plates at high temperatures.
[0007] The object of the invention is achieved in this way:
[0008] A steel for a 1500MPa battery pack for new energy vehicles, the components of the steel being as follows by weight percentage: C: 0.25%-0.27%, Si: 0.20%-0.40%, Al: 0.60%-0.80%, Mn: 1.1%-1.3%, Cr: 0.50%-0.80%, Mo: 0.40%-0.60%, B: 0.004%-0.006%, P≤0.015%, S≤0.003%, Ti: 0.015-0.035%, and the balance being Fe and unavoidable impurities.
[0009] The microstructure of the steel for the battery pack includes critical zone ferrite, tempered martensite and carbide, and the volume percentage of each microstructure is as follows: critical zone ferrite 6% to 10%, tempered martensite 80% to 85%, carbide 1.5% to 2.5% and a small amount of other unidentified phases; preferably, the carbide is mainly θ-type carbide, the volume fraction of θ-type carbide accounts for more than 80% of all carbides, and the average grain size is 45 to 80nm.
[0010] The steel for the battery pack has a tensile strength of more than 1500 MPa, a yield strength of 1200-1350 MPa, an elongation of ≥8%, a hole expansion rate of ≥55%, an isothermal yield decay of less than 300 MPa at 400°C for 5 minutes, and an isothermal yield decay of less than 600 MPa at 800°C for 5 minutes.
[0011] The reasons for the composition design of the present invention are as follows:
[0012] C: C is a necessary element in high-strength steel to ensure the strength of the steel plate. In the present invention, the C addition range is strictly controlled. The addition of C ensures the C behavior in the tempered martensite, the content of θ-type carbides and the grain size. Therefore, in the present invention, C is 0.25% to 0.27%.
[0013] Si: Si is a conventional solid solution strengthening element, which plays a role in strengthening the matrix. In the present invention, the main role of Si is to inhibit the precipitation of carbides in tempered martensite to a certain extent and control the content of carbides between tempered martensite. The invention adopts a low Si design because it effectively controls the surface quality of cold-rolled steel sheets. High Si addition will significantly affect the surface of the steel sheet, forming internal oxidation and grain boundary oxidation layers; in addition, excessive Si addition also seriously affects the surface quality of galvanized steel sheets, forming a "leak plating" phenomenon. Therefore, the Si content of the present invention is 0.20% to 0.40%.
[0014] Mn: Mn is a conventional strengthening element in steel, and the composition system of high-strength steel is mainly based on the C-Mn system. The characteristic of the present invention is that a low Mn design is adopted, because the conventional addition of 2.0% or even more Mn content above 1000MPa level significantly improves the hardenability of the steel plate, leading to the formation of bainite and martensite in the hot coiling stage, which seriously increases the difficulty of cold rolling; furthermore, the composite addition of C and Mn also leads to C / Mn segregation, resulting in excessive edge strength, which also increases the difficulty of cold rolling; therefore, the Mn content is controlled at 1.1% to 1.3% in the present invention.
[0015] Al: Al is usually used as a deoxidizer in steel to regulate the O content in steel; in the present invention, the role of Al is crucial. First, Al is added to replace part of Si, taking into account the surface quality while controlling the carbide precipitation content and carbide state; secondly, Al promotes pearlite spheroidization in the hot coiling stage, inhibits bainite and martensite phase transformations that may be caused by high hardenability, ensures a lower hot rolling reduction, and better goes down to the cold rolling stage; furthermore, Al addition effectively regulates the austenite range and ensures the strength-plastic matching performance of the steel plate. Therefore, in the present invention, Al: 0.60% to 0.80%.
[0016] Cr: Cr is a conventional additive element, which plays a role in solid solution strengthening and improving hardenability similar to Mn; in the present invention, Cr plays a crucial role in replacing Mn to improve hot-rolled edge cracks. Therefore, in the present invention, Cr: 0.50% to 0.80%.
[0017] Mo: Mo is a conventional additive element, which plays a role in solid solution strengthening and improving hardenability similar to Mn; in the present invention, Mo plays a crucial role in replacing Mn to improve hot rolling edge cracks and strengthen the hot rolling surface quality. Therefore, in the present invention, Mo: 0.40% to 0.60%.
[0018] B: B is a crucial element of the present invention. Its main function is to improve the hardenability of the steel plate and prevent the formation of epitaxial hot bodies in the slow cooling and fast cooling stages. B: 0.004% to 0.006%
[0019] Ti: Conventional addition of Ti can capture free N atoms in steel and play a role in fixing N. At the same time, TiN can precipitate during the solidification process and play a role in pinning grain boundaries. Ti(C,N) precipitates during the hot rolling stage and plays a role in pinning the original austenite grain boundaries and refining the original austenite grains. In the present invention, the role of Ti is more important in that it exists in the form of precipitation between tempered martensite, captures H atoms, and resists hydrogen-induced cracking. Therefore, in the present invention, Ti: 0.015~0.035%.
[0020] P: P is a harmful element in steel, and the lower its content, the better. Considering the cost, the content of P is controlled within P≤0.015% in the present invention.
[0021] S: S is a harmful element in steel, and the lower its content, the better. Considering the cost, the content of S in the present invention is controlled to S≤0.003%.
[0022] The second technical solution of the present invention is to provide a method for preparing 1500MPa battery pack steel for new energy vehicles, including smelting, continuous casting, hot rolling, pickling, cold rolling, continuous annealing, and skin pass;
[0023] Continuous Casting:
[0024] Through smelting in a converter, the alloy composition within the above range is obtained, the middle package temperature is 1530-1560℃, the billet drawing speed is 0.6-0.8m / min, and the drawing speed is controlled to prevent the "steel leakage alarm" caused by excessive drawing speed.
[0025] Hot Rolled:
[0026] The heating temperature is between 1260 and 1310℃, and the isothermal temperature is 120 to 160 minutes to ensure the precipitation of Ti atoms, which has a good effect on the solidification of N on the steel plate, and ensures the precipitation of Ti (C, N), which plays a role in pinning the original austenite grain boundary and refining the original austenite grain; the control time range is to prevent the precipitation of TiN from coarsening and causing grain boundary embrittlement on the basis of ensuring full solid solution of elements. The starting rolling temperature is between 1080 and 1130℃, and the final rolling temperature is above 900 to 950℃. The starting rolling temperature ensures the recrystallization behavior of austenite; the final rolling temperature prevents the formation of pro-eutectoid ferrite; then ultra-fast cooling + laminar cooling is carried out, the ultra-fast cooling cooling rate is 5 to 8℃ / s, and the laminar cooling rate is 2-3℃ / s. Ultra-fast cooling prevents the supercooled austenite from quickly transitioning to the low temperature range and prevents excessive element distribution; laminar cold precipitation must be pro-eutectoid ferrite to promote pearlite spheroidization. The coiling temperature is 450-490°C, which inhibits oxidation and the formation of grain boundary oxide layer during this stage and ensures the surface quality of the steel plate.
[0027] Pickling: Remove the iron oxide scale generated on the hot-rolled surface. The pickling speed is 90-110 m / min. Prevent pickling from being too slow to increase production costs, and prevent pickling from being too fast to ensure the surface quality of cold-rolled steel plates.
[0028] Cold rolling: The cold rolling reduction rate is 40% to 58%, ensuring a cold rolling reduction of more than 40% to promote tissue fiberization in the cold rolling configuration; at the same time, prevent the cold rolling reduction rate from being too high, resulting in excessive deformation resistance and difficulty in rolling to the target thickness.
[0029] Continuous galvanizing:
[0030] ① The isothermal heating temperature is between 940 and 960 ° C, and the isothermal time is between 10 and 30 seconds. The isothermal temperature ensures the full austenitization temperature. The isothermal time is strictly controlled to prevent the growth of austenite grains in the critical zone, and to ensure that the austenite phase deformation nucleus is completed and equiaxed.
[0031] ② The slow cooling temperature is 680-740°C, and the slow cooling rate is controlled at 1-3°C / s; the ferrite content is controlled at 6%-10%.
[0032] ③ Rapidly cool to below 500℃ at a cooling rate greater than 45℃ / s to play a pre-cooling role to prevent subsequent large undercooling from causing poor plate shape.
[0033] ④ Quench directly in 80-95℃ water, and then remove the surface oxide scale by pickling.
[0034] ⑤ Reheating: Heat to 450-470℃ at a heating rate of 10-20℃ / s, with an isothermal time of 8-12s. Strictly control the temperature and time to prevent excessive carbide precipitation, thereby reducing the strength of the steel plate.
[0035] ⑥ After galvanizing in a zinc pot, enter the alloying furnace for isothermal treatment at an alloying temperature of 480-490°C for 20-30s. Strictly control the temperature to prevent insufficient Fe content in the coating due to too low a temperature, and ensure that the Zn-Fe layer is mainly composed of δ phase to prevent excessive temperature from causing an increase in carbides and coarsening.
[0036] The beneficial effects of the present invention are:
[0037] (1) The chemical composition of the steel material of the present invention mainly contains C and Mn as the main elements, without obvious precious alloys, and the C content is less than 0.27%, which is conducive to laser welding and resistance spot welding during production and application;
[0038] (2) Make the microstructure distribution more uniform and disperse a large number of θ-type carbides on the matrix, which can effectively improve the yield strength and high temperature softening resistance of the steel plate
[0039] (3) The present invention achieves the force-energy index of both hole expansion performance and high yield strength through low-cost alloy design and ingenious process design. DETAILED DESCRIPTION
[0040] The present invention will be further described below by way of examples.
[0041] According to the component ratio of the technical solution, the embodiment of the present invention performs smelting, continuous casting, hot rolling, pickling, cold rolling, continuous galvanizing and skin passing.
[0042] Hot Rolled:
[0043] Heating temperature 1260 ~ 1310 ℃, isothermal time 120 ~ 160min; rolling temperature 1080 ~ 1130 ℃, final rolling temperature 900 ~ 950 ℃ or above, followed by ultra-fast cooling + laminar cooling, ultra-fast cooling rate 5 ~ 8 ℃ / s, laminar cooling rate 2-3 ℃ / s, coiling temperature 450 ~ 490 ℃;
[0044] Pickling: remove the iron oxide scale generated on the hot-rolled surface, the pickling speed is 90-110m / min;
[0045] Cold rolling: The cold rolling reduction rate is 40% to 58%;
[0046] Continuous galvanizing:
[0047] ① Heating isothermal temperature 940~960℃, isothermal time 10~30s,
[0048] ② Slow cooling temperature 680~740℃, slow cooling rate 1~3℃ / s,
[0049] ③ Rapid cooling to below 500℃ at a cooling rate greater than 45℃ / s,
[0050] ④Then directly enter 80-95℃ water for quenching.
[0051] ⑤ Reheating: Heat to 450-470℃ at a heating rate of 10-20℃ / s, and the isothermal time is 8-12s.
[0052] ⑥ Alloying hot-dip galvanizing: The steel plate is galvanized in a zinc pot and then enters an alloying furnace for isothermal treatment at a temperature of 480 to 490°C for 20 to 30 seconds.
[0053] Furthermore, during the smelting and continuous casting process, the tundish temperature is 1530-1560°C, and the billet drawing speed is 0.6-0.8 m / min.
[0054] The composition of the steel of the present invention is shown in Table 1. The main process parameters of continuous casting and hot rolling of the steel of the present invention are shown in Table 2. The main process parameters of annealing of the steel of the present invention are shown in Table 3. The structure and properties of the steel of the present invention are shown in Table 4.
[0055] Table 1 Composition of steel according to the present invention (wt%)
[0056] Example C Mn Cr Mo Si Al Ti B P S 1 0.26 1.15 0.58 0.25 0.22 0.38 0.034 0.004 0.015 0.001 2 0.25 1.26 0.62 0.24 0.25 0.54 0.028 0.006 0.012 0.002 3 0.25 1.16 0.78 0.21 0.25 0.55 0.019 0.004 0.01 0.001 4 0.27 1.14 0.77 0.33 0.24 0.48 0.022 0.004 0.013 0.001 5 0.26 1.1 0.65 0.34 0.33 0.46 0.021 0.004 0.012 0.003 6 0.25 1.18 0.52 0.39 0.34 0.46 0.028 0.005 0.013 0.001 7 0.26 1.25 0.76 0.22 0.39 0.52 0.027 0.004 0.009 0.001 8 0.25 1.21 0.72 0.25 0.28 0.51 0.025 0.006 0.011 0.001 9 0.27 1.29 0.51 0.33 0.21 0.68 0.023 0.004 0.009 0.003 10 0.25 1.18 0.46 0.38 0.25 0.72 0.032 0.004 0.007 0.001 11 0.25 1.16 0.52 0.36 0.24 0.71 0.027 0.006 0.01 0.003 12 0.27 1.28 0.4 0.39 0.39 0.66 0.025 0.004 0.013 0.001 13 0.26 1.26 0.37 0.28 0.28 0.51 0.023 0.005 0.008 0.001 14 0.25 1.14 0.41 0.21 0.21 0.51 0.019 0.005 0.011 0.002 15 0.26 1.16 0.55 0.22 0.38 0.52 0.016 0.004 0.012 0.001
[0057] Table 2 Main process parameters of continuous casting and hot rolling of steel in the embodiment of the present invention
[0058]
[0059] Table 3 Main process parameters for annealing of steel in the embodiment of the present invention
[0060]
[0061] Table 4 Structure and properties of steel according to the present invention
[0062]
[0063] It can be seen from the above that the microstructure of the steel for battery packs produced by the present invention includes critical zone ferrite, tempered martensite, carbide and a small amount of other unidentified phases; the volume percentage of each microstructure is as follows: critical zone ferrite 6% to 10%, tempered martensite 80% to 85%, carbide 1.5% to 2.5%. The carbides are mainly θ-type carbides, and the volume fraction of θ-type carbides accounts for more than 80% of all carbides, and the average grain size is 45 to 80nm. The tensile strength of the steel for battery packs is above 1500MPa, the yield strength is 1200 to 1350MPa, the elongation is ≥8%, the hole expansion rate is ≥55%, the isothermal yield decay at 400°C for 5 minutes is less than 300MPa, and the isothermal yield decay at 800°C for 5 minutes is less than 600MPa.
[0064] In order to describe the present invention, the present invention is appropriately and fully illustrated by the examples in the above. The above implementation modes are only used to illustrate the present invention, but not to limit the present invention. Ordinary technicians in the relevant technical field can make various changes and modifications without departing from the spirit and scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made should be included in the protection scope of the present invention. The patent protection scope of the present invention should be defined by the claims.
Claims
1. A 1500MPa steel for battery packs for new energy vehicles, characterized in that: The steel has the following components by weight percentage: C: 0.25% to 0.27%, Si: 0.20% to 0.40%, Al: 0.60% to 0.80%, Mn: 1.1% to 1.3%, Cr: 0.50% to 0.80%, Mo: 0.40% to 0.60%, B: 0.004% to 0.006%, P≤0.015%, S≤0.003%, Ti: 0.015% to 0.035%, and the balance is Fe and unavoidable impurities; The microstructure of the steel for the battery pack includes intercritical ferrite, tempered martensite, carbide and a small amount of other unidentified phases; the volume percentage of each microstructure is as follows: intercritical ferrite 6% to 10%, tempered martensite 80% to 85%, carbide 1.5% to 2.5%; the carbide is mainly θ-type carbide, the volume fraction of θ-type carbide accounts for more than 80% of all carbides, and the average grain size is 45 to 80nm; The battery pack steel has a tensile strength of more than 1500MPa, a yield strength of 1200-1350MPa, an elongation of ≥8%, a hole expansion rate of ≥55%, an isothermal yield decay of less than 300MPa at 400°C for 5 minutes, and an isothermal yield decay of less than 600MPa at 800°C for 5 minutes; The method for preparing a 1500MPa battery pack steel for new energy vehicles comprises smelting, continuous casting, hot rolling, pickling, cold rolling, continuous galvanizing, and skin pass; Hot Rolled: Heating temperature 1260 ~ 1310 ℃, isothermal time 120 ~ 160min; rolling temperature 1080 ~ 1130 ℃, final rolling temperature 900 ~ 950 ℃, followed by ultra-fast cooling + laminar cooling, ultra-fast cooling rate 5 ~ 8 ℃ / s, laminar cooling rate 2-3 ℃ / s, coiling temperature 450 ~ 490 ℃; Pickling: remove the iron oxide scale generated on the hot-rolled surface, the pickling speed is 90-110m / min; Cold rolling: The cold rolling reduction rate is 40% to 58%; Continuous galvanizing: ① Heating isothermal temperature 940~960℃, isothermal time 10~30s, ② Slow cooling temperature 680~740℃, slow cooling rate 1~3℃ / s, ③ Rapidly cool to below 500℃ at a cooling rate greater than 45℃ / s, ④Then directly enter 80~95℃ water for quenching, ⑤ Reheating: Heat to 450-470℃ at a heating rate of 10-20℃ / s, isothermal time is 8-12s, ⑥ Alloying hot-dip galvanizing: The steel plate is galvanized in a zinc pot and then enters an alloying furnace for isothermal treatment at a temperature of 480 to 490°C for 20 to 30 seconds.
2. The method for preparing a 1500MPa battery pack steel for new energy vehicles according to claim 1, characterized in that: During the smelting and continuous casting process, the tundish temperature is 1530-1560°C, and the billet drawing speed is 0.6-0.8 m / min.
Citation Information
Patent Citations
Cold-rolled high-strength steel with tensile strength above 1500 MPa and excellent formability and its manufacturing method
CN108018484B
Low-carbon medium-manganese high-residual-austenite high-strength and high-toughness steel and heat treatment method thereof
CN112063931A
High-strength cold rolling transformation induced plasticity steel plate and preparation method thereof
CN102409235A
Production method of ultrahigh strength steel plate for cold forming and steel plate
CN103361547A
Quenched and alloyed galvanized steel plate and manufacturing method thereof
CN106811678A